Home » High Conductivity Copper » C15100 H.C. Copper, Solution Treated & Aged Material Data Sheet
C15100 H.C. Copper Material Data Sheet (Wrought, Solution Treated & Aged)
C15100 Solution Treated Aged Copper Overview
C15100 solution treated aged copper is a wrought high conductivity copper (UNS C15100, EN CW120C), known as h.c. copper. Condition: Solution heat-treated & precipitation hardened. This C15100 solution treated aged copper material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C15100 copper parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C15100 copper parts in-house and inspects them before shipment.
C15100 Designation
Copper Alloy: hc-CuZr(wp) (UNS C15100) Condition Solution heat-treated & precipitation hardened UNS number C15100 EN name CW120C ISO name CuZr JIS (Japanese) name C1500
C15100 Solution Treated Aged Copper Composition detail
Al (aluminum) 0 – 0.005 % Cu (copper) 99.8 – 100 % Fe (iron) 0 – 0.005 % Mn (manganese) 0 – 0.005 % Zr (zirconium) 0.05 – 0.15 %
C15100 Physical properties
C15100 Solution Treated Aged Copper Mechanical properties
Young’s modulus 122 – 128 GPa Specific stiffness 13.6 – 14.3 MN.m/kg Yield strength (elastic limit) 220 – 230 MPa Tensile strength 300 – 320 MPa Specific strength 24.6 – 25.7 kN.m/kg Elongation 34 – 36 % strain Compressive strength 220 – 230 MPa Flexural modulus 122 – 128 GPa Flexural strength (modulus of rupture) 220 – 230 MPa Shear modulus 45.1 – 47.4 GPa Bulk modulus 132 – 138 GPa Poisson’s ratio 0.34 – 0.35 Shape factor 28 Hardness – Vickers 115 – 125 HV Elastic stored energy (springs) 193 – 213 kJ/m3 Fatigue strength at 10^7 cycles 90 – 100 MPa Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles 87.4 – 103 MPa
C15100 Impact & fracture properties
Fracture toughness 50 – 51.4 MPa.m0.5 Toughness (G) 19.8 – 21.3 kJ/m2
C15100 Solution Treated Aged Copper Thermal properties
Melting point 1080 °C Maximum service temperature 300 – 350 °C Minimum service temperature -273 °C Thermal conductivity 390 – 398 W/m.°C Specific heat capacity 383 – 387 J/kg.°C Thermal expansion coefficient 16.8 – 16.9 µstrain/°C Thermal shock resistance 103 – 110 °C Thermal distortion resistance 23.1 – 23.6 MW/m Latent heat of fusion 200 – 208 kJ/kg
C15100 Electrical properties
Electrical resistivity 1.91 – 2.04 µohm.cm Electrical conductivity 84.5 – 90.3 %IACS Temperature dependence of resistivity 5.2 – 5.4 /°C Galvanic potential -0.2 – -0.12 V
C15100 Magnetic properties
Magnetic type Non-magnetic
C15100 Optical, aesthetic and acoustic properties
Transparency Opaque Acoustic velocity 3690 – 3780 m/s Mechanical loss coefficient (tan delta) 7.6e-5 – 8.3e-5
C15100 Processing properties
Metal casting Unsuitable Metal cold forming Excellent Metal hot forming Excellent Metal press forming Excellent Metal deep drawing Limited use Machining speed 29 m/min Weldability Notes: Preheating and post weld heat treatment are not required Poor
C15100 Durability
Water (fresh) Excellent Water (salt) Excellent Weak acids Acceptable Strong acids Unacceptable Weak alkalis Excellent Strong alkalis Excellent Organic solvents Excellent Oxidation at 500C Limited use UV radiation (sunlight) Excellent Galling resistance (adhesive wear) Acceptable Flammability Non-flammable
C15100 Solution Treated Aged Copper Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide Not susceptible
C15100 Notes
C15100 Solution Treated Aged Copper Other notes (s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
C15100 Standards with similar compositions
Europe: CW120C to CEN EN 12163, CW120C to CEN EN 12165, CW120C to CEN EN 12166, CW120C to CEN EN 12167, CW120C to CEN EN 12420Germany: 2.158 to DIN, CuZr to DINJapan: CuZr to JIS Z3234USA: C15000, C15000 to SAE J463, C15100, C15100 to ASTM B747, C15100 to ASTM B888, UNS C15000, UNS C15100Tradenames: AMPCO 910, AMPCOLOY 910, AMZIRC-150, ANSONIA ALLOY C15000, BRIDGEPORT NO. 992, CMW 28, ELBRODUR N4, ELECTRAL CRM 16N, MITSUBISHI MKZ, OLIN C151, OUTOKUMPU ZRK015, PMX ALLOY C15100 (PMX 151), REVERE ZIRCONIUM COPPER, ZIRCONIUM COPPER, ZIRCONIUM COPPER 150, ZIRCONIUM-COPPER 992, ZIRCONIUM-COPPER N-4 (NIPPERT ALLOY N-4)