AISI 1040, annealed, Mechanical properties
| Young’s modulus | 208 | – | 216 | GPa |
| Specific stiffness | 26.5 | – | 27.5 | MN.m/kg |
| Yield strength (elastic limit) | 315 | – | 390 | MPa |
| Tensile strength | 475 | – | 575 | MPa |
| Specific strength | 40.1 | – | 49.7 | kN.m/kg |
| Elongation | 24 | – | 36 | % strain |
| Compressive strength | 315 | – | 390 | MPa |
| Flexural modulus | 208 | – | 216 | GPa |
| Flexural strength (modulus of rupture) | 315 | – | 390 | MPa |
| Shear modulus | 80 | – | 85 | GPa |
| Bulk modulus | 161 | – | 176 | GPa |
| Poisson’s ratio | 0.285 | – | 0.295 | |
| Shape factor | 58 | |||
| Hardness – Vickers | 143 | – | 173 | HV |
| Elastic stored energy (springs) | 236 | – | 355 | kJ/m^3 |
| Fatigue strength at 10^7 cycles | 254 | – | 291 | MPa |
| Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles | 222 | – | 332 | MPa |
| AISI 1040, annealed, Mechanical properties |
MODULUS METAL
Sand Casting in Turkey, Permanent Mold Casting in Turkey, Gravity Die Casting in Turkey, Pressure Die Casting in Turkey, High-Pressure Die Casting in Turkey, Investment Casting in Turkey, Foundry in Turkey, Plastic Injection Molding in Turkey, Press Bending ( Press Brake) Products in Turkey, Laser and Plasma Cutting in Turkey, Welded Construction in Turkey, Heat Treated, CNC Machined Products Manufacturer in Turkey