| Young’s modulus | 205 | – | 215 | GPa |
| Specific stiffness | 26.1 | – | 27.4 | MN.m/kg |
| Yield strength (elastic limit) | 310 | – | 350 | MPa |
| Tensile strength | 395 | – | 490 | MPa |
| Specific strength | 39.5 | – | 44.6 | kN.m/kg |
| Elongation | 28 | – | 43 | % strain |
| Compressive strength | 310 | – | 350 | MPa |
| Flexural modulus | 205 | – | 215 | GPa |
| Flexural strength (modulus of rupture) | 310 | – | 350 | MPa |
| Shear modulus | 79 | – | 84 | GPa |
| Bulk modulus | 158 | – | 175 | GPa |
| Poisson’s ratio | 0.285 | – | 0.295 | |
| Shape factor | 59 | |||
| Hardness – Vickers | 125 | – | 150 | HV |
| Elastic stored energy (springs) | 229 | – | 291 | kJ/m^3 |
| Fatigue strength at 10^7 cycles | 223 | – | 260 | MPa |
| Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles | 192 | – | 302 | MPa |
AISI 1020 Normalized Impact & fracture properties
| Fracture toughness | 43 | – | 63 | MPa.m^0.5 |
| Toughness (G) | 9.08 | – | 18.3 | kJ/m^2 |
AISI 1020 Designation
| AISI 1020 Condition: Normalized | |
| UNS number | G10200 |
| US name | ASTM MT1020, ASTM M1020, ASTM 1020, ASME G10200, ASME G10170, ASME 1017, ~SAE 040 X, Y, Z, ~SAE 035S, ~SAE 035C, ~SAE 035B, ~SAE 035A, ~SAE 035 X, Y, Z, ~ASTM A836, ~ASTM 1018 Class A, ~ASME G10210, ~ASME G10180, ~ASME 1021 |
| EN name | S240GP, ~P355NB, ~P310NB, ~HS15 |
| EN number | ~1.0021 |
| ISO name | ~E235 Quality A, ~CE20E4, ~CC21A |
| GB (Chinese) name | ~ML20Al, ~ML18Mn |
| JIS (Japanese) name | SWRM 20, SWRCH20A, SG 255, ~SWRCH18A, ~STKM12C, ~STKM12B, ~STKM12A, ~SPHT 2 |
MODULUS METAL
Sand Casting in Turkey, Permanent Mold Casting in Turkey, Gravity Die Casting in Turkey, Pressure Die Casting in Turkey, High-Pressure Die Casting in Turkey, Investment Casting in Turkey, Foundry in Turkey, Plastic Injection Molding in Turkey, Press Bending ( Press Brake) Products in Turkey, Laser and Plasma Cutting in Turkey, Welded Construction in Turkey, Heat Treated, CNC Machined Products Manufacturer in Turkey, Additive Manufacturing and 3D Printing in Turkey, Quality Enginering and Inspection Service in Turkey, Manufacturing Inspection Service in Turkey, Quality Engineering and Supplier Quality Engineering Service in Turkey, Supplier Quality Control and Inspection Service in Turkey, Resident Engineering Services in Turkey