AISI 1015 As Rolled Carbon Steel Mechanical Properties

AISI 1015 As rolled Mechanical Properties

Young’s modulus205–215GPa
Specific stiffness26.1–27.4MN.m/kg
Yield strength (elastic limit)280–345MPa
Tensile strength375–465MPa
Specific strength35.7–44kN.m/kg
Elongation31–47% strain
Compressive strength280–345MPa
Flexural modulus205–215GPa
Flexural strength (modulus of rupture)280–345MPa
Shear modulus79–84GPa
Bulk modulus158–175GPa
Poisson’s ratio0.285–0.295 
Shape factor60   
Hardness – Vickers123–143HV
Elastic stored energy (springs)188–281kJ/m^3
Fatigue strength at 10^7 cycles215–251MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles185–292MPa

AISI 1015 As rolled Impact & fracture properties

Fracture toughness42–67        MPa.m^0.5
Toughness (G)8.78–20.5kJ/m^2

Designation: AISI 1015
Condition: As rolled
UNS numberG10150
US nameASTM MT1015, ASTM M1015, ASTM G10170, ASTM 1015, ASME G10150, ~SAE SAE J525, ~SAE SAE J524, ~SAE SAE J356, ~ASTM A822, ~ASTM A214, ~ASTM A2
EN nameHS17, ~UkSt37-2, ~P235T1, ~C15R, ~C15E, ~C15
EN number~1.1141, ~1.1140, ~1.0124
ISO name~R33, ~CE15E4, ~CC15X, ~CC15A
GB (Chinese) name~ML15Al, ~CRB650
JIS (Japanese) nameSWRM 17, SWRM 15, SWRCH17R, SWRCH15R, SGD 3, ~SWRCH15A

MODULUS METAL
Sand Casting in Turkey, Permanent Mold Casting in Turkey, Gravity Die Casting in Turkey, Pressure Die Casting in Turkey, High-Pressure Die Casting in Turkey, Investment Casting in Turkey, Foundry in Turkey, Plastic Injection Molding in Turkey, Press Bending ( Press Brake) Products in Turkey, Laser and Plasma Cutting in Turkey, Welded Construction in Turkey, Heat Treated, CNC Machined Products Manufacturer in Turkey, Additive Manufacturing and 3D Printing in Turkey, Quality Enginering and Inspection Service in Turkey, Manufacturing Inspection Service in Turkey, Quality Engineering and Supplier Quality Engineering Service in Turkey, Supplier Quality Control and Inspection Service in Turkey, Resident Engineering Services in Turkey