AISI 1340 Oil Quenched & Tempered at 650°C Material Data Sheet
AISI 1340 Oil Quenched & Tempered at 650°C Overview
| AISI 1340 oil quenched tempered 650°C is AISI 1340 medium carbon manganese steel (UNS G13400, EN 38Mn6) in the oil quenched & tempered at 650°C condition. This AISI 1340 oil quenched tempered 650°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 1340 conditions in our AISI 1340 yield, tensile and hardness comparison. Looking for AISI 1340 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1340 steel parts in-house and inspects them before shipment. |
AISI 1340 Oil Quenched & Tempered at 650°C Designation
| AISI 1340 | |
| Condition | Tempered at 650°C & oil quenched |
| UNS number | G13400, ~H13400 |
| EN name | BS S 156, BS S 157, 38Mn6 |
| EN number | 1.1127 |
AISI 1340 Oil Quenched & Tempered at 650°C Typical uses
| General construction, general mechanical engineering, automotive, tools, axles, gears, springs. |
AISI 1340 Oil Quenched & Tempered at 650°C Composition detail
| C (carbon) | 0.38 | – | 0.43 | % |
| Fe (iron) | 97.2 | – | 97.9 | % |
| Mn (manganese) | 1.6 | – | 1.9 | % |
| P (phosphorus) | 0 | – | 0.035 | % |
| S (sulfur) | 0 | – | 0.04 | % |
| Si (silicon) | 0.15 | – | 0.35 | % |
AISI 1340 Oil Quenched & Tempered at 650°C Physical properties
| Density | 7.8 | – | 7.9 | g/cm3 |
AISI 1340 Oil Quenched & Tempered at 650°C Mechanical properties
| Young’s modulus | 200 | – | 215 | GPa |
| Specific stiffness | 25.5 | – | 27.4 | MN.m/kg |
| Yield strength (elastic limit) | 555 | – | 690 | MPa |
| Tensile strength | 720 | – | 880 | MPa |
| Specific strength | 70.7 | – | 87.9 | kN.m/kg |
| Elongation | 17 | – | 27 | % strain |
| Compressive strength | 555 | – | 690 | MPa |
| Flexural modulus | 200 | – | 215 | GPa |
| Flexural strength (modulus of rupture) | 555 | – | 690 | MPa |
| Shear modulus | 77 | – | 84 | GPa |
| Bulk modulus | 155 | – | 175 | GPa |
| Poisson’s ratio | 0.285 | – | 0.295 | |
| Shape factor | 40 | |||
| Hardness – Vickers | 230 | – | 280 | HV |
| Elastic stored energy (springs) | 749 | – | 1140 | kJ/m3 |
| Fatigue strength at 10^7 cycles | 340 | – | 392 | MPa |
| Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles | 297 | – | 450 | MPa |
AISI 1340 Oil Quenched & Tempered at 650°C Impact & fracture properties
| Fracture toughness | 33 | – | 56 | MPa.m0.5 |
| Toughness (G) | 5.55 | – | 14.3 | kJ/m2 |
AISI 1340 Oil Quenched & Tempered at 650°C Thermal properties
| Melting point | 1430 | – | 1500 | °C |
| Maximum service temperature | 323 | – | 349 | °C |
| Minimum service temperature | -53 | – | -23 | °C |
| Thermal conductivity | 45 | – | 55 | W/m.°C |
| Specific heat capacity | 440 | – | 520 | J/kg.°C |
| Thermal expansion coefficient | 11 | – | 13 | µstrain/°C |
| Thermal shock resistance | 217 | – | 287 | °C |
| Thermal distortion resistance | 3.66 | – | 4.73 | MW/m |
| Latent heat of fusion | 270 | – | 275 | kJ/kg |
AISI 1340 Oil Quenched & Tempered at 650°C Electrical properties
| Electrical resistivity | 15 | – | 22 | µohm.cm |
| Electrical conductivity | 7.84 | – | 11.5 | %IACS |
| Galvanic potential | -0.52 | – | -0.44 | V |
AISI 1340 Oil Quenched & Tempered at 650°C Magnetic properties
| Magnetic type | Magnetic |
AISI 1340 Oil Quenched & Tempered at 650°C Optical, aesthetic and acoustic properties
| Transparency | Opaque | |||
| Acoustic velocity | 5050 | – | 5240 | m/s |
| Mechanical loss coefficient (tan delta) | 5.3e-4 | – | 6.7e-4 | |
AISI 1340 Oil Quenched & Tempered at 650°C Processing properties
| Metal casting | Unsuitable |
| Metal cold forming | Acceptable |
| Metal hot forming | Acceptable |
| Metal press forming | Acceptable |
| Metal deep drawing | Limited use |
| Machining speed | 21.3 m/min |
| Weldability Notes: Preheating and post weld heat treatments may be required | Good |
| Carbon equivalency | 0.647 – 0.747 |
AISI 1340 Oil Quenched & Tempered at 650°C Durability
| Water (fresh) | Acceptable |
| Water (salt) | Limited use |
| Weak acids | Limited use |
| Strong acids | Unacceptable |
| Weak alkalis | Acceptable |
| Strong alkalis | Limited use |
| Organic solvents | Excellent |
| Oxidation at 500C | Acceptable |
| UV radiation (sunlight) | Excellent |
| Galling resistance (adhesive wear) Notes: Aluminum bronze is the most suitable mating material to minimize galling. | Acceptable |
| Flammability | Non-flammable |
AISI 1340 Oil Quenched & Tempered at 650°C Corrosion resistance
| Stress corrosion cracking Note: Rated in chloride; Other susceptible environments: Nitrate, hydroxide, carbonate, ammonia | Slightly susceptible |
AISI 1340 Oil Quenched & Tempered at 650°C Standards with similar compositions
| Australia: K1340 to AS 1442, X1340 to AS 1442, X1340 to AS 1443, X1345 to AS 1442 |
| China: 45Mn2 to GB/T 11251 |
| France: 40M6 to AFNOR NF A35-552 |
| Germany: 36Mn6 to DIN, 46Mn7 to DIN |
| India: 37C15 to IS 11169/1, 37C15 to IS 13352, 37C15 to IS 9175/15, 37Mn2 to IS 4368 |
| International: 36Mn6 to ISO 683-1, 36Mn6 to ISO 683-18, 42Mn6 to ISO 683-1, 42Mn6 to ISO 683-18, 42Mn6E to ISO 4954 |
| Japan: SMn 2 to JIS G4106, SMn 3 to JIS G4106, SMn2H to JIS G4052, SMn3H to JIS G4052, SWRCH41K to JIS G3507 |
| Mexico: 1335 to NMX-B-300, 1340 to NMX-B-203-SCFI, 1340 to NMX-B-300, 1340H to NMX-B-300, 1345 to NMX-B-203-SCFI, 1345 to NMX-B-300, 1345H to NMX-B-268, 1345H to NMX-B-300, 1541 to NMX-B-301 |
| Pan America: 1335 to COPANT 514, 1340 to COPANT 334, 1340 to COPANT 514, 1345 to COPANT 514 |
| South Korea: SMn 438 H to KS D 3754, SMn 438 to KS D 3724, SMn 443 H to KS D 3754, SMn 443 to KS D 3724, SWRCH41K to KS D 3592 |
| USA: 1335, 1335 to ASTM A29/A29M, 1335 to ASTM A331-95, 1335 to ASTM A519, 1335 to ASTM A829/A829M, 1335 to DoD-F-24669/1, 1335 to MIL-S-16974E, 1335 to SAE J404, 1335 to SAE J770, 1340, 1340 to ASTM A29/A29M, 1340 to ASTM A331-95, 1340 to ASTM A513, 1340 to ASTM A519, 1340 to ASTM A829/A829M, 1340 to MIL-S-16974E, 1340 to SAE J404, 1340 to SAE J770, 1345, 1345 to ASTM A29/A29M, 1345 to ASTM A331-95, 1345 to ASTM A519, 1345 to ASTM A829/A829M, 1345 to FED QQ-S-626C, 1345 to SAE J404, 1345 to SAE J770, 1541H, 1541H to ASTM A304, 1541H to SAE J1268, 15B41H, 15B41H to ASTM A304, 15B41H to SAE J1268, 15L41H, E1541H, G15410 to ASTM A830/A830M, H15410 to SAE J775, NV1 to SAE J775, UNS G13350, UNS G13400, UNS G13450, UNS H13350, UNS H13400, UNS H13450, UNS H15410, UNS H15411 |
| Tradenames: A-1203, AR, AR-235 (1), BOHLER V742, COLFORM E.T.D. 1541 A, COLFORM E.T.D. 1541 B, INTERMEDIATE MANGANESE ABRASION STEEL, KAISALOY AR, KRUPP 36 MN 6, KRUPP 46 MN 7, POMPEY 1541, ROC 250, SHEFFIELD-AR, XK1335, XK1340, XK1345 |