AISI 1340 Oil Quenched & Tempered at 315°C Material Data Sheet

AISI 1340 Oil Quenched & Tempered at 315°C Material Data Sheet

AISI 1340 Oil Quenched & Tempered at 315°C Overview

AISI 1340 oil quenched tempered 315°C is AISI 1340 medium carbon manganese steel (UNS G13400, EN 38Mn6) in the oil quenched & tempered at 315°C condition. This AISI 1340 oil quenched tempered 315°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 1340 conditions in our AISI 1340 yield, tensile and hardness comparison. Looking for AISI 1340 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1340 steel parts in-house and inspects them before shipment.

AISI 1340 Oil Quenched & Tempered at 315°C Designation

AISI 1340
ConditionTempered at 315°C & oil quenched
UNS numberG13400, ~H13400
EN nameBS S 156, BS S 157, 38Mn6
EN number1.1127

AISI 1340 Oil Quenched & Tempered at 315°C Typical uses

General construction, general mechanical engineering, automotive, tools, axles, gears, springs.

AISI 1340 Oil Quenched & Tempered at 315°C Composition detail

C (carbon)0.38–0.43%
Fe (iron)97.2–97.9%
Mn (manganese)1.6–1.9%
P (phosphorus)0–0.035%
S (sulfur)0–0.04%
Si (silicon)0.15–0.35%

AISI 1340 Oil Quenched & Tempered at 315°C Physical properties

Density7.8–7.9g/cm3

AISI 1340 Oil Quenched & Tempered at 315°C Mechanical properties

Young’s modulus200–215GPa
Specific stiffness25.5–27.4MN.m/kg
Yield strength (elastic limit)1280–1570MPa
Tensile strength1430–1750MPa
Specific strength162–199kN.m/kg
Elongation9–15% strain
Compressive strength1270–1570MPa
Flexural modulus200–215GPa
Flexural strength (modulus of rupture)1280–1570MPa
Shear modulus77–84GPa
Bulk modulus155–175GPa
Poisson’s ratio0.285–0.295 
Shape factor17
Hardness – Vickers408–498HV
Elastic stored energy (springs)3950–5860kJ/m3
Fatigue strength at 10^7 cycles548–634MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
478–726MPa

AISI 1340 Oil Quenched & Tempered at 315°C Impact & fracture properties

Fracture toughness15–31MPa.m0.5
Toughness (G)1.2–4.21kJ/m2

AISI 1340 Oil Quenched & Tempered at 315°C Thermal properties

Melting point1430–1500°C
Maximum service temperature275–305°C
Minimum service temperature-18–12°C
Thermal conductivity45–55W/m.°C
Specific heat capacity440–520J/kg.°C
Thermal expansion coefficient11–13µstrain/°C
Thermal shock resistance498–651°C
Thermal distortion resistance3.66–4.73MW/m
Latent heat of fusion270–275kJ/kg

AISI 1340 Oil Quenched & Tempered at 315°C Electrical properties

Electrical resistivity15–22µohm.cm
Electrical conductivity7.84–11.5%IACS
Galvanic potential-0.52–-0.44V

AISI 1340 Oil Quenched & Tempered at 315°C Magnetic properties

Magnetic typeMagnetic

AISI 1340 Oil Quenched & Tempered at 315°C Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5050–5240m/s
Mechanical loss coefficient (tan delta)2.5e-4–3.2e-4 

AISI 1340 Oil Quenched & Tempered at 315°C Processing properties

Metal castingUnsuitable
Metal cold formingAcceptable
Metal hot formingAcceptable
Metal press formingAcceptable
Metal deep drawingLimited use
Machining speed11 m/min
Weldability
Notes: Preheating and post weld heat treatments may be required
Good
Carbon equivalency0.647 – 0.747

AISI 1340 Oil Quenched & Tempered at 315°C Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Aluminum bronze is the most suitable mating material to minimize galling.
Acceptable
FlammabilityNon-flammable

AISI 1340 Oil Quenched & Tempered at 315°C Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; Other susceptible environments: Nitrate, hydroxide, carbonate, ammonia
Susceptible

AISI 1340 Oil Quenched & Tempered at 315°C Standards with similar compositions

Australia: K1340 to AS 1442, X1340 to AS 1442, X1340 to AS 1443, X1345 to AS 1442
China: 45Mn2 to GB/T 11251
France: 40M6 to AFNOR NF A35-552
Germany: 36Mn6 to DIN, 46Mn7 to DIN
India: 37C15 to IS 11169/1, 37C15 to IS 13352, 37C15 to IS 9175/15, 37Mn2 to IS 4368
International: 36Mn6 to ISO 683-1, 36Mn6 to ISO 683-18, 42Mn6 to ISO 683-1, 42Mn6 to ISO 683-18, 42Mn6E to ISO 4954
Japan: SMn 2 to JIS G4106, SMn 3 to JIS G4106, SMn2H to JIS G4052, SMn3H to JIS G4052, SWRCH41K to JIS G3507
Mexico: 1335 to NMX-B-300, 1340 to NMX-B-203-SCFI, 1340 to NMX-B-300, 1340H to NMX-B-300, 1345 to NMX-B-203-SCFI, 1345 to NMX-B-300, 1345H to NMX-B-268, 1345H to NMX-B-300, 1541 to NMX-B-301
Pan America: 1335 to COPANT 514, 1340 to COPANT 334, 1340 to COPANT 514, 1345 to COPANT 514
South Korea: SMn 438 H to KS D 3754, SMn 438 to KS D 3724, SMn 443 H to KS D 3754, SMn 443 to KS D 3724, SWRCH41K to KS D 3592
USA: 1335, 1335 to ASTM A29/A29M, 1335 to ASTM A331-95, 1335 to ASTM A519, 1335 to ASTM A829/A829M, 1335 to DoD-F-24669/1, 1335 to MIL-S-16974E, 1335 to SAE J404, 1335 to SAE J770, 1340, 1340 to ASTM A29/A29M, 1340 to ASTM A331-95, 1340 to ASTM A513, 1340 to ASTM A519, 1340 to ASTM A829/A829M, 1340 to MIL-S-16974E, 1340 to SAE J404, 1340 to SAE J770, 1345, 1345 to ASTM A29/A29M, 1345 to ASTM A331-95, 1345 to ASTM A519, 1345 to ASTM A829/A829M, 1345 to FED QQ-S-626C, 1345 to SAE J404, 1345 to SAE J770, 1541H, 1541H to ASTM A304, 1541H to SAE J1268, 15B41H, 15B41H to ASTM A304, 15B41H to SAE J1268, 15L41H, E1541H, G15410 to ASTM A830/A830M, H15410 to SAE J775, NV1 to SAE J775, UNS G13350, UNS G13400, UNS G13450, UNS H13350, UNS H13400, UNS H13450, UNS H15410, UNS H15411
Tradenames: A-1203, AR, AR-235 (1), BOHLER V742, COLFORM E.T.D. 1541 A, COLFORM E.T.D. 1541 B, INTERMEDIATE MANGANESE ABRASION STEEL, KAISALOY AR, KRUPP 36 MN 6, KRUPP 46 MN 7, POMPEY 1541, ROC 250, SHEFFIELD-AR, XK1335, XK1340, XK1345