AISI 12L14 As Rolled Material Data Sheet

AISI 12L14 As Rolled Material Data Sheet

AISI 12L14 As Rolled Overview

AISI 12L14 as rolled is AISI 12L14 leaded resulfurized low carbon steel (UNS G12144, EN 11SMnPb37) in the as rolled condition. This AISI 12L14 as rolled material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. See also the resulfurized free-machining steels comparison. Looking for AISI 12L14 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 12L14 steel parts in-house and inspects them before shipment.

AISI 12L14 As Rolled Designation

AISI 12L14
ConditionAs rolled
UNS numberG12144
US nameAISI 12L14, 12L13, 12L15 to ASTM A29, ASTM A510, ASTM A519, ASTM A576, SAE J403
EN name11SMnPb37, 11SMnPb30, 9SMnPb28 to BS EN 10087, BS EN 10277; S300Pb to NF A35 561
EN number1.0737, 1.0718, 1.9718
JIS (Japanese) nameSUM24L to JIS G4804
TradenamesLEDLOY 1214, Usaled, AMER-LED

AISI 12L14 As Rolled Typical uses

Free-machining / free-cutting steel for automatic screw machine and tool products, shafts, bolts, fasteners, cams, lightly stressed fasteners, for the automotive and general engineering industries.

AISI 12L14 As Rolled Composition detail

C (carbon)0–0.15%
Fe (iron)97.8–98.7%
Mn (manganese)0.85–1.15%
P (phosphorus)0.04–0.09%
Pb (lead)0.15–0.35%
S (sulfur)0.26–0.35%
Si (silicon)0–0.1%

AISI 12L14 As Rolled Physical properties

Density7.83–7.91g/cm3

AISI 12L14 As Rolled Mechanical properties

Young’s modulus196–204GPa
Specific stiffness24.9–25.9MN.m/kg
Yield strength (elastic limit)342–517MPa
Tensile strength380–570MPa
Specific strength43.5–65.7kN.m/kg
Elongation10–17% strain
Compressive strength342–517MPa
Flexural modulus196–204GPa
Flexural strength (modulus of rupture)276–322MPa
Shear modulus77.7–82.4GPa
Bulk modulus152–168GPa
Poisson’s ratio0.29
Shape factor52
Hardness – Vickers115–250HV
Hardness – Rockwell B68–84HRB
Hardness – Brinell121–174HB
Elastic stored energy (springs)303–645kJ/m3
Fatigue strength at 10^7 cycles171–199MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
126–269MPa

AISI 12L14 As Rolled Impact & fracture properties

Fracture toughness76–92MPa.m0.5
Toughness (G)29.1–42kJ/m2

AISI 12L14 As Rolled Thermal properties

Melting point1490–1530°C
Maximum service temperature343–357°C
Minimum service temperature-63–-38°C
Thermal conductivity52–55W/m.°C
Specific heat capacity460–472J/kg.°C
Thermal expansion coefficient11.5  µstrain/°C
Thermal shock resistance149–225°C
Thermal distortion resistance4.52–4.78MW/m
Latent heat of fusion270–275kJ/kg

AISI 12L14 As Rolled Electrical properties

Electrical resistivity12–17.4µohm.cm
Electrical conductivity9.91–14.4%IACS
Galvanic potential-0.52–-0.44V

AISI 12L14 As Rolled Magnetic properties

Magnetic typeMagnetic

AISI 12L14 As Rolled Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity4990–5090m/s

AISI 12L14 As Rolled Processing properties

Metal castingUnsuitable
Metal cold formingAcceptable
Metal hot formingExcellent
Metal press formingAcceptable
Metal deep drawingUnsuitable
Machining speed45.7 m/min
Weldability
Notes: Preheating and post weld heat treatments may be required, and contains hazardous elements
Poor
Weldability – TIGNot recommended
Carbon equivalency0.028 – 0.192

AISI 12L14 As Rolled Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Aluminum bronze is the most suitable mating material to minimize galling.
Acceptable
FlammabilityNon-flammable

AISI 12L14 As Rolled Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; Other susceptible environments: Nitrate, hydroxide, carbonate, ammonia
Slightly susceptible