AISI 1080 Oil Quenched & Tempered at 540°C Material Data Sheet

AISI 1080 Oil Quenched & Tempered at 540°C Material Data Sheet

AISI 1080 Oil Quenched & Tempered at 540°C Overview

AISI 1080 oil quenched tempered 540°C is AISI 1080 high carbon steel (UNS G10800) in the oil quenched & tempered at 540°C condition. This AISI 1080 oil quenched tempered 540°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 1080 conditions in our AISI 1080 yield, tensile and hardness comparison. Looking for AISI 1080 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1080 steel parts in-house and inspects them before shipment.

AISI 1080 Oil Quenched & Tempered at 540°C Designation

AISI 1080
ConditionTempered at 540°C & oil quenched
UNS numberG10800
US nameASTM Class C, ASTM 1080, ASME G10800, ~ASTM G10780, ~ASTM 1078
EN name~HS80

AISI 1080 Oil Quenched & Tempered at 540°C Typical uses

General construction, general mechanical engineering, automotive, tools, axles, gears, springs.

AISI 1080 Oil Quenched & Tempered at 540°C Composition detail

C (carbon)0.75–0.88%
Fe (iron)98.1–98.6%
Mn (manganese)0.6–0.9%
P (phosphorus)0–0.04%
S (sulfur)0–0.05%

AISI 1080 Oil Quenched & Tempered at 540°C Physical properties

Density7.8–7.9g/cm3

AISI 1080 Oil Quenched & Tempered at 540°C Mechanical properties

Young’s modulus200–215GPa
Specific stiffness25.5–27.4MN.m/kg
Yield strength (elastic limit)725–890MPa
Tensile strength1020–1250MPa
Specific strength92.3–113kN.m/kg
Elongation13–19% strain
Compressive strength725–890MPa
Flexural modulus200–215GPa
Flexural strength (modulus of rupture)725–890MPa
Shear modulus77–84GPa
Bulk modulus155–175GPa
Poisson’s ratio0.285–0.295 
Shape factor31
Hardness – Vickers300–350HV
Elastic stored energy (springs)1280–1900kJ/m3
Fatigue strength at 10^7 cycles432–501MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
377–575MPa

AISI 1080 Oil Quenched & Tempered at 540°C Impact & fracture properties

Fracture toughness33–56MPa.m0.5
Toughness (G)5.55–14.3kJ/m2

AISI 1080 Oil Quenched & Tempered at 540°C Thermal properties

Melting point1330–1480°C
Maximum service temperature286–340°C
Minimum service temperature-38–-8°C
Thermal conductivity48–53W/m.°C
Specific heat capacity470–510J/kg.°C
Thermal expansion coefficient11–12.5µstrain/°C
Thermal shock resistance292–374°C
Thermal distortion resistance3.97–4.66MW/m
Latent heat of fusion270–275kJ/kg

AISI 1080 Oil Quenched & Tempered at 540°C Electrical properties

Electrical resistivity17–20µohm.cm
Electrical conductivity8.62–10.1%IACS
Galvanic potential-0.51–-0.43V

AISI 1080 Oil Quenched & Tempered at 540°C Magnetic properties

Magnetic typeMagnetic

AISI 1080 Oil Quenched & Tempered at 540°C Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5050–5240m/s
Mechanical loss coefficient (tan delta)3.9e-4–4.9e-4 

AISI 1080 Oil Quenched & Tempered at 540°C Processing properties

Metal castingUnsuitable
Metal cold formingLimited use
Metal hot formingLimited use
Metal press formingAcceptable
Metal deep drawingLimited use
Machining speed14.6 m/min
Weldability
Notes: Preheating and post weld heat treatments may be required
Good
Carbon equivalency0.85 – 1.03

AISI 1080 Oil Quenched & Tempered at 540°C Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Aluminum bronze is the most suitable mating material to minimize galling.
Acceptable
FlammabilityNon-flammable

AISI 1080 Oil Quenched & Tempered at 540°C Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; Other susceptible environments: Nitrate, hydroxide, carbonate, ammonia
Slightly susceptible

AISI 1080 Oil Quenched & Tempered at 540°C Standards with similar compositions

India: 75C6 to IS 1570/2/1, 80C6 to IS 1570/2/1, 85C6 to IS 1570/2/1, C75 to IS 1570/2/1, C80 to IS 1570/2/1, C85 to IS 1570/2/1
Mexico: 1074 to NMX-B-301, 1080 to NMX-B-301, 1084 to NMX-B-301, 1085 to NMX-B-301
Pan America: 1080 to COPANT 330, 1080 to COPANT 331
USA: 1074, 1074 to ASTM A29/A29M, 1074 to ASTM A568/A568M, 1074 to ASTM A713, 1074 to SAE J403, 1080, 1080 to ASTM A29/A29M, 1080 to ASTM A568/A568M, 1080 to ASTM A713, 1080 to DoD-F-24669/1, 1080 to FED QQ-W-470B, 1080 to MIL-S-16974E, 1080 to SAE J403, 1084, 1084 to ASTM A29/A29M, 1084 to ASTM A568/A568M, 1084 to ASTM A713, 1084 to SAE J1249, 1084 to SAE J403, 1085, 1085 to ASTM A568/A568M, 1085 to SAE J403, 1090, 1090 to ASTM A568/A568M, 1090 to SAE J403, 1580, 1580 to SAE J403, C1080 to FED QQ-S-700D, C1084 to FED QQ-S-700D, C8 to MIL-S-16788A, G10740 to ASTM A510/A510M, G10800 to ASTM A510/A510M, G10800 to ASTM A576-90b, G10840 to ASTM A510/A510M, G10840 to ASTM A576-90b, G10850 to ASTM A510/A510M, UNS G10740, UNS G10740 to UNS, UNS G10800, UNS G10800 to UNS, UNS G10840, UNS G10840 to UNS, UNS G10850, UNS G10900, UNS G15800
Tradenames: B/82, BOHLER NAB, DISSTON NO. 5390, FIRTH-BROWN F75C, FORTUNA HSB2, FORTUNA W83K, INGERSOLL I-75, INGERSOLL I-85, KRUPP W 93, S/83, SANDVIK 13LM, SODERFORS ANVIL, SPEAR 75, TULIPE EXTRA NO. 4, VEW B908