AISI 1080 Oil Quenched & Tempered at 425°C Material Data Sheet
AISI 1080 Oil Quenched & Tempered at 425°C Overview
| AISI 1080 oil quenched tempered 425°C is AISI 1080 high carbon steel (UNS G10800) in the oil quenched & tempered at 425°C condition. This AISI 1080 oil quenched tempered 425°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 1080 conditions in our AISI 1080 yield, tensile and hardness comparison. Looking for AISI 1080 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1080 steel parts in-house and inspects them before shipment. |
AISI 1080 Oil Quenched & Tempered at 425°C Designation
| AISI 1080 | |
| Condition | Tempered at 425°C & oil quenched |
| UNS number | G10800 |
| US name | ASTM Class C, ASTM 1080, ASME G10800, ~ASTM G10780, ~ASTM 1078 |
| EN name | ~HS80 |
AISI 1080 Oil Quenched & Tempered at 425°C Typical uses
| General construction, general mechanical engineering, automotive, tools, axles, gears, springs. |
AISI 1080 Oil Quenched & Tempered at 425°C Composition detail
| C (carbon) | 0.75 | – | 0.88 | % |
| Fe (iron) | 98.1 | – | 98.6 | % |
| Mn (manganese) | 0.6 | – | 0.9 | % |
| P (phosphorus) | 0 | – | 0.04 | % |
| S (sulfur) | 0 | – | 0.05 | % |
AISI 1080 Oil Quenched & Tempered at 425°C Physical properties
| Density | 7.8 | – | 7.9 | g/cm3 |
AISI 1080 Oil Quenched & Tempered at 425°C Mechanical properties
| Young’s modulus | 200 | – | 215 | GPa |
| Specific stiffness | 25.5 | – | 27.4 | MN.m/kg |
| Yield strength (elastic limit) | 855 | – | 1050 | MPa |
| Tensile strength | 1160 | – | 1430 | MPa |
| Specific strength | 109 | – | 133 | kN.m/kg |
| Elongation | 11 | – | 15 | % strain |
| Compressive strength | 855 | – | 1050 | MPa |
| Flexural modulus | 200 | – | 215 | GPa |
| Flexural strength (modulus of rupture) | 855 | – | 1050 | MPa |
| Shear modulus | 77 | – | 84 | GPa |
| Bulk modulus | 155 | – | 175 | GPa |
| Poisson’s ratio | 0.285 | – | 0.295 | |
| Shape factor | 26 | |||
| Hardness – Vickers | 350 | – | 410 | HV |
| Elastic stored energy (springs) | 1770 | – | 2620 | kJ/m3 |
| Fatigue strength at 10^7 cycles | 473 | – | 549 | MPa |
| Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles | 412 | – | 630 | MPa |
AISI 1080 Oil Quenched & Tempered at 425°C Impact & fracture properties
| Fracture toughness | 28 | – | 50 | MPa.m0.5 |
| Toughness (G) | 4.03 | – | 11.3 | kJ/m2 |
AISI 1080 Oil Quenched & Tempered at 425°C Thermal properties
| Melting point | 1330 | – | 1480 | °C |
| Maximum service temperature | 286 | – | 340 | °C |
| Minimum service temperature | -33 | – | -3 | °C |
| Thermal conductivity | 48 | – | 53 | W/m.°C |
| Specific heat capacity | 470 | – | 510 | J/kg.°C |
| Thermal expansion coefficient | 11 | – | 12.5 | µstrain/°C |
| Thermal shock resistance | 344 | – | 439 | °C |
| Thermal distortion resistance | 3.97 | – | 4.66 | MW/m |
| Latent heat of fusion | 270 | – | 275 | kJ/kg |
AISI 1080 Oil Quenched & Tempered at 425°C Electrical properties
| Electrical resistivity | 17 | – | 20 | µohm.cm |
| Electrical conductivity | 8.62 | – | 10.1 | %IACS |
| Galvanic potential | -0.51 | – | -0.43 | V |
AISI 1080 Oil Quenched & Tempered at 425°C Magnetic properties
| Magnetic type | Magnetic |
AISI 1080 Oil Quenched & Tempered at 425°C Optical, aesthetic and acoustic properties
| Transparency | Opaque | |||
| Acoustic velocity | 5050 | – | 5240 | m/s |
| Mechanical loss coefficient (tan delta) | 3.4e-4 | – | 4.3e-4 | |
AISI 1080 Oil Quenched & Tempered at 425°C Processing properties
| Metal casting | Unsuitable |
| Metal cold forming | Limited use |
| Metal hot forming | Limited use |
| Metal press forming | Acceptable |
| Metal deep drawing | Limited use |
| Machining speed | 12.5 m/min |
| Weldability Notes: Preheating and post weld heat treatments may be required | Good |
| Carbon equivalency | 0.85 – 1.03 |
AISI 1080 Oil Quenched & Tempered at 425°C Durability
| Water (fresh) | Acceptable |
| Water (salt) | Limited use |
| Weak acids | Limited use |
| Strong acids | Unacceptable |
| Weak alkalis | Acceptable |
| Strong alkalis | Limited use |
| Organic solvents | Excellent |
| Oxidation at 500C | Acceptable |
| UV radiation (sunlight) | Excellent |
| Galling resistance (adhesive wear) Notes: Aluminum bronze is the most suitable mating material to minimize galling. | Acceptable |
| Flammability | Non-flammable |
AISI 1080 Oil Quenched & Tempered at 425°C Corrosion resistance
| Stress corrosion cracking Note: Rated in chloride; Other susceptible environments: Nitrate, hydroxide, carbonate, ammonia | Slightly susceptible |
AISI 1080 Oil Quenched & Tempered at 425°C Standards with similar compositions
| India: 75C6 to IS 1570/2/1, 80C6 to IS 1570/2/1, 85C6 to IS 1570/2/1, C75 to IS 1570/2/1, C80 to IS 1570/2/1, C85 to IS 1570/2/1 |
| Mexico: 1074 to NMX-B-301, 1080 to NMX-B-301, 1084 to NMX-B-301, 1085 to NMX-B-301 |
| Pan America: 1080 to COPANT 330, 1080 to COPANT 331 |
| USA: 1074, 1074 to ASTM A29/A29M, 1074 to ASTM A568/A568M, 1074 to ASTM A713, 1074 to SAE J403, 1080, 1080 to ASTM A29/A29M, 1080 to ASTM A568/A568M, 1080 to ASTM A713, 1080 to DoD-F-24669/1, 1080 to FED QQ-W-470B, 1080 to MIL-S-16974E, 1080 to SAE J403, 1084, 1084 to ASTM A29/A29M, 1084 to ASTM A568/A568M, 1084 to ASTM A713, 1084 to SAE J1249, 1084 to SAE J403, 1085, 1085 to ASTM A568/A568M, 1085 to SAE J403, 1090, 1090 to ASTM A568/A568M, 1090 to SAE J403, 1580, 1580 to SAE J403, C1080 to FED QQ-S-700D, C1084 to FED QQ-S-700D, C8 to MIL-S-16788A, G10740 to ASTM A510/A510M, G10800 to ASTM A510/A510M, G10800 to ASTM A576-90b, G10840 to ASTM A510/A510M, G10840 to ASTM A576-90b, G10850 to ASTM A510/A510M, UNS G10740, UNS G10740 to UNS, UNS G10800, UNS G10800 to UNS, UNS G10840, UNS G10840 to UNS, UNS G10850, UNS G10900, UNS G15800 |
| Tradenames: B/82, BOHLER NAB, DISSTON NO. 5390, FIRTH-BROWN F75C, FORTUNA HSB2, FORTUNA W83K, INGERSOLL I-75, INGERSOLL I-85, KRUPP W 93, S/83, SANDVIK 13LM, SODERFORS ANVIL, SPEAR 75, TULIPE EXTRA NO. 4, VEW B908 |