AISI 1015 Normalized Material Data Sheet

AISI 1015 Normalized Material Data Sheet

AISI 1015 Normalized Overview

AISI 1015 normalized is AISI 1015 low carbon steel (UNS G10150) in the normalized condition. This AISI 1015 normalized material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 1015 conditions in our AISI 1015 yield, tensile and hardness comparison. Looking for AISI 1015 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1015 steel parts in-house and inspects them before shipment.

AISI 1015 Normalized Designation

AISI 1015
ConditionNormalized
UNS numberG10150
US nameASTM MT1015, ASTM M1015, ASTM G10170, ASTM 1015, ASME G10150, ~SAE SAE J525, ~SAE SAE J524, ~SAE SAE J356, ~ASTM A822, ~ASTM A214, ~ASTM A2
EN nameHS17, ~UkSt37-2, ~P235T1, ~C15R, ~C15E, ~C15
EN number~1.1141, ~1.1140, ~1.0124
ISO name~R33, ~CE15E4, ~CC15X, ~CC15A
GB (Chinese) name~ML15Al, ~CRB650
JIS (Japanese) nameSWRM 17, SWRM 15, SWRCH17R, SWRCH15R, SGD 3, ~SWRCH15A

AISI 1015 Normalized Typical uses

General construction, general mechanical engineering, automotive, tools, axles, gears, springs.

AISI 1015 Normalized Composition detail

C (carbon)0.13–0.18%
Fe (iron)99.1–99.6%
Mn (manganese)0.3–0.6%
P (phosphorus)0–0.04%
S (sulfur)0–0.05%

AISI 1015 Normalized Physical properties

Density7.8–7.9g/cm3

AISI 1015 Normalized Mechanical properties

Young’s modulus205–215GPa
Specific stiffness26.1–27.4MN.m/kg
Yield strength (elastic limit)300–355MPa
Tensile strength380–470MPa
Specific strength38.2–45.2kN.m/kg
Elongation29–45% strain
Compressive strength300–355MPa
Flexural modulus205–215GPa
Flexural strength (modulus of rupture)300–355MPa
Shear modulus79–84GPa
Bulk modulus158–175GPa
Poisson’s ratio0.285–0.295 
Shape factor59
Hardness – Vickers118–138HV
Elastic stored energy (springs)215–299kJ/m3
Fatigue strength at 10^7 cycles217–253MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
187–294MPa

AISI 1015 Normalized Impact & fracture properties

Fracture toughness41–63MPa.m0.5
Toughness (G)8.31–18.2kJ/m2

AISI 1015 Normalized Thermal properties

Melting point1490–1530°C
Maximum service temperature344–357°C
Minimum service temperature-68–-43°C
Thermal conductivity50–54W/m.°C
Specific heat capacity465–505J/kg.°C
Thermal expansion coefficient11.5–13µstrain/°C
Thermal shock resistance114–141°C
Thermal distortion resistance3.96–4.57MW/m
Latent heat of fusion270–275kJ/kg

AISI 1015 Normalized Electrical properties

Electrical resistivity16–18µohm.cm
Electrical conductivity9.58–10.8%IACS
Galvanic potential-0.52–-0.44V

AISI 1015 Normalized Magnetic properties

Magnetic typeMagnetic

AISI 1015 Normalized Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5110–5240m/s
Mechanical loss coefficient (tan delta)0.00102–0.00125 

AISI 1015 Normalized Processing properties

Metal castingUnsuitable
Metal cold formingAcceptable
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingAcceptable
Machining speed42.7 m/min
Weldability
Notes: Preheating and post weld heat treatments may be required
Excellent
Carbon equivalency0.18 – 0.28

AISI 1015 Normalized Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Aluminum bronze is the most suitable mating material to minimize galling.
Acceptable
FlammabilityNon-flammable

AISI 1015 Normalized Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; Other susceptible environments: Nitrate, hydroxide, carbonate, ammonia
Not susceptible

AISI 1015 Normalized Standards with similar compositions

China: ML15Al to GB/T 6478
India: 12C5 to IS 8053, 14C4 to IS 1871/2, 14C6 to IS 11169/1, 14C6 to IS 1570/2/1, C14 to IS 1570/2/1, C15Mn75 to IS 6967, CDS-2 to IS 3074, Fe 310 to IS 12367, Grade 6 to IS 7887, Grade 6 to IS 8952, Grade 7 to IS 7887, Grade 7 to IS 8952
International: CC15A to ISO 4954, CC15X to ISO 4954
Japan: SGD 3 to JIS G3108, SWRCH15A to JIS G3507, SWRCH15R to JIS G3507, SWRCH17R to JIS G3507, SWRM 15 to JIS G3505, SWRM 17 to JIS G3505
Mexico: 1015 to NMX-B-301, 1017 to NMX-B-301, MT1015 to NMX-B-201, MT1015 to NMX-B-203-SCFI
Pan America: 1015 to COPANT 330, 1015 to COPANT 331, 1015 to COPANT 333, 1017 to COPANT 333
South Korea: SGD 3 to KS D 3526, SWRCH15A to KS D 3592, SWRCH15R to KS D 3592, SWRCH17R to KS D 3592, SWRM 15 to KS D 3554, SWRM 17 to KS D 3554
Spain: 16KA-DF to UNE 36032, F.7515 to UNE 36032
UK: 040A17 to BS 970/1, HS17 to BS 1449 Section 1.14
USA: 1013 to SAE J403, 1015, 1015 to ASTM A29/A29M, 1015 to ASTM A512-96, 1015 to ASTM A513, 1015 to ASTM A519, 1015 to ASTM A568/A568M, 1015 to ASTM A787, 1015 to DoD-F-24669/1, 1015 to FED QQ-S-698, 1015 to FED QQ-W-461H, 1015 to MIL-T-3520, 1015 to SAE J403, 1017, 1017 to ASTM A29/A29M, 1017 to ASTM A513, 1017 to ASTM A519, 1017 to ASTM A568/A568M, 1017 to ASTM A787, 1017 to SAE J403, 5061 to AMS 5061E, G10150 to ASTM A510/A510M, G10150 to ASTM A576-90b, G10150 to ASTM A830/A830M, G10170 to ASTM A510/A510M, G10170 to ASTM A576-90b, G10170 to ASTM A830/A830M, Grade B to ASTM A31, Grade C to ASTM A1020/A1020M, Grade C to ASTM A178/A178M, Grade C to ASTM A285/A285M, M1015, M1015 to ASTM A29/A29M, M1015 to ASTM A575-96, M1015 to SAE J403, M1017, M1017 to ASTM A29/A29M, M1017 to ASTM A575-96, MT1015 to ASTM A512-96, MT1015 to ASTM A513, MT1015 to ASTM A519, MT1015 to ASTM A787, UNS G10150, UNS G10150 to UNS, UNS G10170, UNS G10170 to UNS, UNS K00802, UNS K01602, UNS K02801, UNS K03003, UNS K03007, UNS K03100, UNS K03503
Tradenames: AMERCUT C-1115, DEEPEX, FORTUNA W23, JESSOP A-2A, JESSOP STEEL A-2, MARTINSITE M130, MARTINSITE M160, MARTINSITE M190, MARTINSITE M220, PREMIER EB WELD, PREMIER EP WELD, SHARALLOY 50, SHARALLOY 55, SHARALLOY 60, SPANG CHALFANT 2, TIMKEN CARBON, UNA HIGH SPEED NO. 45, UNA HIGH TENSILE NO. 65, UNA NO. 160, UNA NO. 300, V1, YO-FLEX 60, YO-FLEX 70, YO-FLEX 80, YO-FLEX 90