AISI 1015 As Rolled Material Data Sheet
AISI 1015 As Rolled Overview
| AISI 1015 as rolled is AISI 1015 low carbon steel (UNS G10150) in the as rolled condition. This AISI 1015 as rolled material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 1015 conditions in our AISI 1015 yield, tensile and hardness comparison. Looking for AISI 1015 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1015 steel parts in-house and inspects them before shipment. |
AISI 1015 As Rolled Designation
| AISI 1015 | |
| Condition | As rolled |
| UNS number | G10150 |
| US name | ASTM MT1015, ASTM M1015, ASTM G10170, ASTM 1015, ASME G10150, ~SAE SAE J525, ~SAE SAE J524, ~SAE SAE J356, ~ASTM A822, ~ASTM A214, ~ASTM A2 |
| EN name | HS17, ~UkSt37-2, ~P235T1, ~C15R, ~C15E, ~C15 |
| EN number | ~1.1141, ~1.1140, ~1.0124 |
| ISO name | ~R33, ~CE15E4, ~CC15X, ~CC15A |
| GB (Chinese) name | ~ML15Al, ~CRB650 |
| JIS (Japanese) name | SWRM 17, SWRM 15, SWRCH17R, SWRCH15R, SGD 3, ~SWRCH15A |
AISI 1015 As Rolled Typical uses
| General construction, general mechanical engineering, automotive, tools, axles, gears, springs. |
AISI 1015 As Rolled Composition detail
| C (carbon) | 0.13 | – | 0.18 | % |
| Fe (iron) | 99.1 | – | 99.6 | % |
| Mn (manganese) | 0.3 | – | 0.6 | % |
| P (phosphorus) | 0 | – | 0.04 | % |
| S (sulfur) | 0 | – | 0.05 | % |
AISI 1015 As Rolled Physical properties
| Density | 7.8 | – | 7.9 | g/cm3 |
AISI 1015 As Rolled Mechanical properties
| Young’s modulus | 205 | – | 215 | GPa |
| Specific stiffness | 26.1 | – | 27.4 | MN.m/kg |
| Yield strength (elastic limit) | 280 | – | 345 | MPa |
| Tensile strength | 375 | – | 465 | MPa |
| Specific strength | 35.7 | – | 44 | kN.m/kg |
| Elongation | 31 | – | 47 | % strain |
| Compressive strength | 280 | – | 345 | MPa |
| Flexural modulus | 205 | – | 215 | GPa |
| Flexural strength (modulus of rupture) | 280 | – | 345 | MPa |
| Shear modulus | 79 | – | 84 | GPa |
| Bulk modulus | 158 | – | 175 | GPa |
| Poisson’s ratio | 0.285 | – | 0.295 | |
| Shape factor | 60 | |||
| Hardness – Vickers | 123 | – | 143 | HV |
| Elastic stored energy (springs) | 188 | – | 281 | kJ/m3 |
| Fatigue strength at 10^7 cycles | 215 | – | 251 | MPa |
| Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles | 185 | – | 292 | MPa |
AISI 1015 As Rolled Impact & fracture properties
| Fracture toughness | 42 | – | 67 | MPa.m0.5 |
| Toughness (G) | 8.78 | – | 20.5 | kJ/m2 |
AISI 1015 As Rolled Thermal properties
| Melting point | 1490 | – | 1530 | °C |
| Maximum service temperature | 344 | – | 357 | °C |
| Minimum service temperature | -68 | – | -43 | °C |
| Thermal conductivity | 50 | – | 54 | W/m.°C |
| Specific heat capacity | 465 | – | 505 | J/kg.°C |
| Thermal expansion coefficient | 11.5 | – | 13 | µstrain/°C |
| Thermal shock resistance | 107 | – | 137 | °C |
| Thermal distortion resistance | 3.96 | – | 4.57 | MW/m |
| Latent heat of fusion | 270 | – | 275 | kJ/kg |
AISI 1015 As Rolled Electrical properties
| Electrical resistivity | 16 | – | 18 | µohm.cm |
| Electrical conductivity | 9.58 | – | 10.8 | %IACS |
| Galvanic potential | -0.52 | – | -0.44 | V |
AISI 1015 As Rolled Magnetic properties
| Magnetic type | Magnetic |
AISI 1015 As Rolled Optical, aesthetic and acoustic properties
| Transparency | Opaque | |||
| Acoustic velocity | 5110 | – | 5240 | m/s |
| Mechanical loss coefficient (tan delta) | 0.00104 | – | 0.0013 | |
AISI 1015 As Rolled Processing properties
| Metal casting | Unsuitable |
| Metal cold forming | Acceptable |
| Metal hot forming | Excellent |
| Metal press forming | Excellent |
| Metal deep drawing | Acceptable |
| Machining speed | 39.6 m/min |
| Weldability Notes: Preheating and post weld heat treatments may be required | Excellent |
| Carbon equivalency | 0.18 – 0.28 |
AISI 1015 As Rolled Durability
| Water (fresh) | Acceptable |
| Water (salt) | Limited use |
| Weak acids | Limited use |
| Strong acids | Unacceptable |
| Weak alkalis | Acceptable |
| Strong alkalis | Limited use |
| Organic solvents | Excellent |
| Oxidation at 500C | Acceptable |
| UV radiation (sunlight) | Excellent |
| Galling resistance (adhesive wear) Notes: Aluminum bronze is the most suitable mating material to minimize galling. | Acceptable |
| Flammability | Non-flammable |
AISI 1015 As Rolled Corrosion resistance
| Stress corrosion cracking Note: Rated in chloride; Other susceptible environments: Nitrate, hydroxide, carbonate, ammonia | Not susceptible |
AISI 1015 As Rolled Standards with similar compositions
| China: ML15Al to GB/T 6478 |
| India: 12C5 to IS 8053, 14C4 to IS 1871/2, 14C6 to IS 11169/1, 14C6 to IS 1570/2/1, C14 to IS 1570/2/1, C15Mn75 to IS 6967, CDS-2 to IS 3074, Fe 310 to IS 12367, Grade 6 to IS 7887, Grade 6 to IS 8952, Grade 7 to IS 7887, Grade 7 to IS 8952 |
| International: CC15A to ISO 4954, CC15X to ISO 4954 |
| Japan: SGD 3 to JIS G3108, SWRCH15A to JIS G3507, SWRCH15R to JIS G3507, SWRCH17R to JIS G3507, SWRM 15 to JIS G3505, SWRM 17 to JIS G3505 |
| Mexico: 1015 to NMX-B-301, 1017 to NMX-B-301, MT1015 to NMX-B-201, MT1015 to NMX-B-203-SCFI |
| Pan America: 1015 to COPANT 330, 1015 to COPANT 331, 1015 to COPANT 333, 1017 to COPANT 333 |
| South Korea: SGD 3 to KS D 3526, SWRCH15A to KS D 3592, SWRCH15R to KS D 3592, SWRCH17R to KS D 3592, SWRM 15 to KS D 3554, SWRM 17 to KS D 3554 |
| Spain: 16KA-DF to UNE 36032, F.7515 to UNE 36032 |
| UK: 040A17 to BS 970/1, HS17 to BS 1449 Section 1.14 |
| USA: 1013 to SAE J403, 1015, 1015 to ASTM A29/A29M, 1015 to ASTM A512-96, 1015 to ASTM A513, 1015 to ASTM A519, 1015 to ASTM A568/A568M, 1015 to ASTM A787, 1015 to DoD-F-24669/1, 1015 to FED QQ-S-698, 1015 to FED QQ-W-461H, 1015 to MIL-T-3520, 1015 to SAE J403, 1017, 1017 to ASTM A29/A29M, 1017 to ASTM A513, 1017 to ASTM A519, 1017 to ASTM A568/A568M, 1017 to ASTM A787, 1017 to SAE J403, 5061 to AMS 5061E, G10150 to ASTM A510/A510M, G10150 to ASTM A576-90b, G10150 to ASTM A830/A830M, G10170 to ASTM A510/A510M, G10170 to ASTM A576-90b, G10170 to ASTM A830/A830M, Grade B to ASTM A31, Grade C to ASTM A1020/A1020M, Grade C to ASTM A178/A178M, Grade C to ASTM A285/A285M, M1015, M1015 to ASTM A29/A29M, M1015 to ASTM A575-96, M1015 to SAE J403, M1017, M1017 to ASTM A29/A29M, M1017 to ASTM A575-96, MT1015 to ASTM A512-96, MT1015 to ASTM A513, MT1015 to ASTM A519, MT1015 to ASTM A787, UNS G10150, UNS G10150 to UNS, UNS G10170, UNS G10170 to UNS, UNS K00802, UNS K01602, UNS K02801, UNS K03003, UNS K03007, UNS K03100, UNS K03503 |
| Tradenames: AMERCUT C-1115, DEEPEX, FORTUNA W23, JESSOP A-2A, JESSOP STEEL A-2, MARTINSITE M130, MARTINSITE M160, MARTINSITE M190, MARTINSITE M220, PREMIER EB WELD, PREMIER EP WELD, SHARALLOY 50, SHARALLOY 55, SHARALLOY 60, SPANG CHALFANT 2, TIMKEN CARBON, UNA HIGH SPEED NO. 45, UNA HIGH TENSILE NO. 65, UNA NO. 160, UNA NO. 300, V1, YO-FLEX 60, YO-FLEX 70, YO-FLEX 80, YO-FLEX 90 |