PPA 33% Glass Fiber (Polyphthalamide) Material Data Sheet
PPA 33% Glass Fiber Overview
PPA 33% glass fiber is a grade of polyphthalamide (PPA), designated Polyphthalamide (33% glass fiber). This PPA 33% glass fiber material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PPA parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PPA parts in-house and inspects them before shipment.
PPA 33% Glass Fiber Designation
Polyphthalamide (33% glass fiber)
Tradenames
Amodel, Edgetek, Grivory, Zytel
PPA 33% Glass Fiber Typical uses
Industrial and chemical processing equipment, bearings, gears, electrical connectors, packaging, under bonnet automobile applications
PPA 33% Glass Fiber Composition detail
Polymer
67
%
Glass (fiber)
33
%
PPA 33% Glass Fiber Physical properties
Density
1.46
–
1.49
g/cm3
PPA 33% Glass Fiber Mechanical properties
Young’s modulus
10.9
–
13.6
GPa
Specific stiffness
7.39
–
9.22
MN.m/kg
Yield strength (elastic limit)
166
–
207
MPa
Tensile strength
168
–
205
MPa
Specific strength
113
–
140
kN.m/kg
Elongation
1.74
–
2.51
% strain
Elongation at yield
1.47
–
2.78
% strain
Compressive modulus
11.6
–
12.9
GPa
Compressive strength
212
–
235
MPa
Flexural modulus
10.1
–
12.1
GPa
Flexural strength (modulus of rupture)
223
–
273
MPa
Shear modulus
4.4
–
4.63
GPa
Shear strength
71.7
–
87.6
MPa
Bulk modulus
13.5
–
14.9
GPa
Poisson’s ratio
0.343
–
0.356
Shape factor
6.23
Hardness – Vickers
53
–
59
HV
Hardness – Rockwell M
184
–
204
Hardness – Rockwell R
184
–
204
Hardness – Shore D
98
–
102
Elastic stored energy (springs)
1120
–
1780
kJ/m3
Fatigue strength at 10^7 cycles
70.8
–
78.2
MPa
PPA 33% Glass Fiber Impact & fracture properties
Fracture toughness
5.07
–
5.61
MPa.m0.5
Toughness (G)
2.02
–
2.7
kJ/m2
Impact strength, notched 23 °C
5.95
–
11.6
kJ/m2
Impact strength, notched -30 °C
5.51
–
12
kJ/m2
Impact strength, unnotched 23 °C
45.6
–
66.9
kJ/m2
Impact strength, unnotched -30 °C
44
–
66
kJ/m2
PPA 33% Glass Fiber Thermal properties
Melting point
299
–
322
°C
Glass temperature
119
–
135
°C
Heat deflection temperature 0.45MPa
284
–
340
°C
Heat deflection temperature 1.8MPa
258
–
313
°C
Maximum service temperature
215
–
235
°C
Minimum service temperature
-49
–
-29
°C
Thermal conductivity
0.458
–
0.474
W/m.°C
Specific heat capacity
1360
–
1410
J/kg.°C
Thermal expansion coefficient
23
–
58
µstrain/°C
Thermal shock resistance
259
–
671
°C
Thermal distortion resistance
0.00803
–
0.0203
MW/m
PPA 33% Glass Fiber Electrical properties
Electrical resistivity
1.55e18
–
3.87e19
µohm.cm
Electrical conductivity
4.46e-18
–
1.11e-16
%IACS
Dielectric constant (relative permittivity)
3.93
–
5.54
Dissipation factor (dielectric loss tangent)
0.00542
–
0.0143
Dielectric strength (dielectric breakdown)
25.3
–
43.2
MV/m
Comparative tracking index
575
–
600
V
PPA 33% Glass Fiber Magnetic properties
Magnetic type
Non-magnetic
PPA 33% Glass Fiber Optical, aesthetic and acoustic properties