PARA 50% Glass Fiber Material Data Sheet

PARA 50% Glass Fiber (Polyarylamide) Material Data Sheet

PARA 50% Glass Fiber Overview

PARA 50% glass fiber is a grade of polyarylamide (PARA), designated Polyarylamide (50% glass fiber). This PARA 50% glass fiber material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PARA parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PARA parts in-house and inspects them before shipment.

PARA 50% Glass Fiber Designation

Polyarylamide (50% glass fiber)
TradenamesGlamide, Ixef, Reny

PARA 50% Glass Fiber Typical uses

Automotive, furniture, small appliances, lawn mowers, power tools, electrical contactors and switches, medical devices, electrical motor components, cell phones, faucet components.

PARA 50% Glass Fiber Composition detail

Polymer50–54%
Glass (fiber)46–50%

PARA 50% Glass Fiber Physical properties

Density1.63–1.66g/cm3

PARA 50% Glass Fiber Mechanical properties

Young’s modulus17.8–22.2GPa
Specific stiffness10.8–13.5MN.m/kg
Yield strength (elastic limit)231–289MPa
Tensile strength234–286MPa
Specific strength140–176kN.m/kg
Elongation1.8–2.6% strain
Elongation at yield1.52–2.88% strain
Compressive modulus19–21GPa
Compressive strength296–328MPa
Flexural modulus16.5–19.8GPa
Flexural strength (modulus of rupture)354–433MPa
Shear modulus7.31–7.68GPa
Shear strength140–172MPa
Bulk modulus19.1–21.1GPa
Poisson’s ratio0.329–0.334 
Shape factor6.88
Hardness – Vickers74–82HV
Hardness – Rockwell M184–204 
Hardness – Rockwell R184–204 
Hardness – Shore D98–102 
Elastic stored energy (springs)1330–2120kJ/m3
Fatigue strength at 10^7 cycles98.8–109MPa

PARA 50% Glass Fiber Impact & fracture properties

Fracture toughness5.6–6.19MPa.m0.5
Toughness (G)1.51–2.01kJ/m2
Impact strength, notched 23 °C6.19–12kJ/m2
Impact strength, unnotched 23 °C45.7–67.2kJ/m2

PARA 50% Glass Fiber Thermal properties

Melting point269–291°C
Glass temperature77.8–92.2°C
Heat deflection temperature 0.45MPa247–268°C
Heat deflection temperature 1.8MPa220–240°C
Vicat softening point77–90°C
Maximum service temperature193–207°C
Thermal conductivity0.598–0.636W/m.°C
Specific heat capacity1670–1730J/kg.°C
Thermal expansion coefficient14.5–16.5µstrain/°C
Thermal shock resistance713–991°C
Thermal distortion resistance0.0371–0.0428MW/m

PARA 50% Glass Fiber Electrical properties

Electrical resistivity2e20–5e21µohm.cm
Electrical conductivity3.45e-20–8.62e-19%IACS
Dielectric constant (relative permittivity)4.05–5.71 
Dissipation factor (dielectric loss tangent)0.0205–0.054 
Dielectric strength (dielectric breakdown)22–37.4MV/m
Comparative tracking index600  V

PARA 50% Glass Fiber Magnetic properties

Magnetic typeNon-magnetic

PARA 50% Glass Fiber Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3280–3680m/s
Mechanical loss coefficient (tan delta)0.0059–0.00652 

PARA 50% Glass Fiber Absorption & permeability

Water absorption @ 24 hrs0.12–0.2%
Water absorption @ sat2.8–3.8%
Humidity absorption @ sat0.78–1.1%

PARA 50% Glass Fiber Processing properties

Polymer injection moldingLimited use
Polymer extrusionAcceptable
Polymer thermoformingLimited use
Linear mold shrinkage0.1 – 0.3 %
Melt temperature269 – 291 °C
Mold temperature120 – 140 °C
Molding pressure range30 – 150 MPa

PARA 50% Glass Fiber Durability

Water (fresh)Excellent
Water (salt)Acceptable
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsLimited use
Oils and fuelsAcceptable
Oxidation at 500CUnacceptable
UV radiation (sunlight)Good
FlammabilitySlow-burning