PARA 60% Glass Fiber Material Data Sheet

PARA 60% Glass Fiber (Polyarylamide) Material Data Sheet

PARA 60% Glass Fiber Overview

PARA 60% glass fiber is a grade of polyarylamide (PARA), designated Polyarylamide (60% glass fiber). This PARA 60% glass fiber material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PARA parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PARA parts in-house and inspects them before shipment.

PARA 60% Glass Fiber Designation

Polyarylamide (60% glass fiber)
TradenamesIxef, Reny

PARA 60% Glass Fiber Typical uses

Automotive, furniture, small appliances, lawn mowers, power tools, electrical contactors and switches, electrical motor components, cell phones, faucet components.

PARA 60% Glass Fiber Composition detail

Polymer40  %
Glass (fiber)60  %

PARA 60% Glass Fiber Physical properties

Density1.77–1.81g/cm3

PARA 60% Glass Fiber Mechanical properties

Young’s modulus20.5–25.5GPa
Specific stiffness11.4–14.3MN.m/kg
Yield strength (elastic limit)223–278MPa
Tensile strength225–275MPa
Specific strength125–155kN.m/kg
Elongation1.64–2.36% strain
Elongation at yield1.38–2.62% strain
Compressive modulus21.9–24.2GPa
Compressive strength285–315MPa
Flexural modulus20.7–24.8GPa
Flexural strength (modulus of rupture)340–416MPa
Shear modulus8.46–8.89GPa
Shear strength135–165MPa
Bulk modulus20.9–23.1GPa
Poisson’s ratio0.324–0.326 
Shape factor7.7
Hardness – Vickers71–80HV
Hardness – Rockwell M184–204 
Hardness – Rockwell R184–204 
Hardness – Shore D98–102 
Elastic stored energy (springs)1080–1710kJ/m3
Fatigue strength at 10^7 cycles95–105MPa

PARA 60% Glass Fiber Impact & fracture properties

Fracture toughness5.76–6.37MPa.m0.5
Toughness (G)1.39–1.85kJ/m2
Impact strength, notched 23 °C7.41–14.4kJ/m2
Impact strength, unnotched 23 °C45.7–67.2kJ/m2

PARA 60% Glass Fiber Thermal properties

Melting point269–291°C
Glass temperature78–92.2°C
Heat deflection temperature 0.45MPa247–268°C
Heat deflection temperature 1.8MPa220–240°C
Vicat softening point77–90°C
Maximum service temperature188–207°C
Thermal conductivity0.672–0.691W/m.°C
Specific heat capacity1570–1630J/kg.°C
Thermal expansion coefficient13.7–14.4µstrain/°C
Thermal shock resistance667–907°C
Thermal distortion resistance0.0473–0.0501MW/m

PARA 60% Glass Fiber Electrical properties

Electrical resistivity2e20–5e21µohm.cm
Electrical conductivity3.45e-20–8.62e-19%IACS
Dielectric constant (relative permittivity)3.96–5.59 
Dissipation factor (dielectric loss tangent)0.0108–0.0286 
Dielectric strength (dielectric breakdown)17.6–30MV/m
Comparative tracking index600  V

PARA 60% Glass Fiber Magnetic properties

Magnetic typeNon-magnetic

PARA 60% Glass Fiber Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3380–3780m/s
Mechanical loss coefficient (tan delta)0.00527–0.00583 

PARA 60% Glass Fiber Absorption & permeability

Water absorption @ 24 hrs0.099–0.16%
Water absorption @ sat2.4–3.2%
Humidity absorption @ sat0.68–0.92%

PARA 60% Glass Fiber Processing properties

Polymer injection moldingLimited use
Polymer extrusionAcceptable
Polymer thermoformingLimited use
Linear mold shrinkage0.1 – 0.3 %
Melt temperature269 – 291 °C
Mold temperature122 – 138 °C
Molding pressure range30 – 150 MPa

PARA 60% Glass Fiber Durability

Water (fresh)Excellent
Water (salt)Acceptable
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsLimited use
Oils and fuelsAcceptable
Oxidation at 500CUnacceptable
UV radiation (sunlight)Good
FlammabilitySlow-burning