PARA 50% Glass Fiber Flame Retarded Material Data Sheet
PARA 50% Glass Fiber Flame Retarded (Polyarylamide) Material Data Sheet
PARA 50% Glass Fiber Flame Retarded Overview
PARA 50% glass fiber flame retarded is a grade of polyarylamide (PARA), designated Polyarylamide (50% glass fiber, flame retarded). This PARA 50% glass fiber flame retarded material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PARA parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PARA parts in-house and inspects them before shipment.
PARA 50% Glass Fiber Flame Retarded Designation
Polyarylamide (50% glass fiber, flame retarded)
Tradenames
Ixef, Reny
PARA 50% Glass Fiber Flame Retarded Typical uses
Automotive, furniture, small appliances, lawn mowers, power tools, electrical contactors and switches, electrical motor components, cell phones, faucet components.
PARA 50% Glass Fiber Flame Retarded Composition detail
Polymer
35
–
45
%
Flame retardant
5
–
15
%
Glass (fiber)
50
%
PARA 50% Glass Fiber Flame Retarded Physical properties
Density
1.75
–
1.79
g/cm3
PARA 50% Glass Fiber Flame Retarded Mechanical properties
Young’s modulus
17
–
21.2
GPa
Specific stiffness
9.6
–
12
MN.m/kg
Yield strength (elastic limit)
172
–
215
MPa
Tensile strength
182
–
222
MPa
Specific strength
97.1
–
122
kN.m/kg
Elongation
1.8
–
2.59
% strain
Elongation at yield
1.52
–
2.88
% strain
Compressive modulus
18.1
–
20
GPa
Compressive strength
230
–
254
MPa
Flexural modulus
16.6
–
19.9
GPa
Flexural strength (modulus of rupture)
272
–
333
MPa
Shear modulus
6.97
–
7.33
GPa
Shear strength
109
–
133
MPa
Bulk modulus
18
–
19.9
GPa
Poisson’s ratio
0.327
–
0.332
Shape factor
8.11
Hardness – Vickers
55
–
61
HV
Hardness – Rockwell M
184
–
204
Hardness – Rockwell R
184
–
204
Hardness – Shore D
98
–
102
Elastic stored energy (springs)
771
–
1230
kJ/m3
Fatigue strength at 10^7 cycles
76.7
–
84.7
MPa
PARA 50% Glass Fiber Flame Retarded Impact & fracture properties
Fracture toughness
5.55
–
6.13
MPa.m0.5
Toughness (G)
1.55
–
2.07
kJ/m2
Impact strength, notched 23 °C
6.66
–
12.9
kJ/m2
Impact strength, unnotched 23 °C
28
–
41.2
kJ/m2
PARA 50% Glass Fiber Flame Retarded Thermal properties
Melting point
268
–
282
°C
Glass temperature
78
–
92.2
°C
Heat deflection temperature 0.45MPa
254
–
258
°C
Heat deflection temperature 1.8MPa
226
–
230
°C
Vicat softening point
77
–
90
°C
Maximum service temperature
187
–
199
°C
Thermal conductivity
0.629
–
0.644
W/m.°C
Specific heat capacity
1160
–
1180
J/kg.°C
Thermal expansion coefficient
16.6
–
17.4
µstrain/°C
Thermal shock resistance
510
–
696
°C
Thermal distortion resistance
0.0364
–
0.0385
MW/m
PARA 50% Glass Fiber Flame Retarded Electrical properties
Electrical resistivity
2e20
–
5e21
µohm.cm
Electrical conductivity
3.45e-20
–
8.62e-19
%IACS
Dielectric constant (relative permittivity)
3.62
–
5.1
Dissipation factor (dielectric loss tangent)
0.0145
–
0.0381
Dielectric strength (dielectric breakdown)
21.3
–
36.2
MV/m
Comparative tracking index
400
–
450
V
PARA 50% Glass Fiber Flame Retarded Magnetic properties
Magnetic type
Non-magnetic
PARA 50% Glass Fiber Flame Retarded Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
3090
–
3470
m/s
Mechanical loss coefficient (tan delta)
0.00588
–
0.0065
PARA 50% Glass Fiber Flame Retarded Absorption & permeability
Water absorption @ 24 hrs
0.17
–
0.28
%
Water absorption @ sat
1.4
–
1.9
%
Humidity absorption @ sat
1
–
1.4
%
PARA 50% Glass Fiber Flame Retarded Processing properties