PARA 20% Glass Fiber Wear Grade Overview

PARA 20% glass fiber wear grade is a grade of polyarylamide (PARA), designated Polyarylamide (20% glass fiber, wear grade). This PARA 20% glass fiber wear grade material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PARA parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PARA parts in-house and inspects them before shipment.

PARA 20% Glass Fiber Wear Grade Designation

Polyarylamide (20% glass fiber, wear grade)
TradenamesReny

PARA 20% Glass Fiber Wear Grade Typical uses

Automotive, furniture, small appliances, lawn mowers, power tools, electrical contactors and switches, electrical motor components, cell phones, faucet components.

PARA 20% Glass Fiber Wear Grade Composition detail

Polymer80  %
Glass (fiber)20  %

PARA 20% Glass Fiber Wear Grade Physical properties

Density1.5–1.53g/cm3

PARA 20% Glass Fiber Wear Grade Mechanical properties

Young’s modulus7.2–8.98GPa
Specific stiffness4.75–5.93MN.m/kg
Yield strength (elastic limit)95.3–119MPa
Tensile strength107–130MPa
Specific strength62.9–78.6kN.m/kg
Elongation2.22–3.2% strain
Elongation at yield1.87–3.55% strain
Compressive modulus7.69–8.49GPa
Compressive strength135–149MPa
Flexural modulus5.94–7.11GPa
Flexural strength (modulus of rupture)154–188MPa
Shear modulus2.92–3.07GPa
Shear strength63.9–78.2MPa
Bulk modulus8.66–9.57GPa
Poisson’s ratio0.35–0.352 
Shape factor6.8
Hardness – Vickers31–34HV
Hardness – Rockwell M157–174 
Hardness – Rockwell R157–174 
Hardness – Shore D92–96 
Elastic stored energy (springs)559–890kJ/m3
Fatigue strength at 10^7 cycles45–49.7MPa

PARA 20% Glass Fiber Wear Grade Impact & fracture properties

Fracture toughness4.67–5.16MPa.m0.5
Toughness (G)2.59–3.46kJ/m2
Impact strength, notched 23 °C4.76–9.24kJ/m2
Impact strength, unnotched 23 °C35–38kJ/m2

PARA 20% Glass Fiber Wear Grade Thermal properties

Melting point269–291°C
Glass temperature78–92.2°C
Heat deflection temperature 0.45MPa237–258°C
Heat deflection temperature 1.8MPa210–230°C
Vicat softening point77–90°C
Maximum service temperature188–207°C
Thermal conductivity0.471–0.482W/m.°C
Specific heat capacity1310–1340J/kg.°C
Thermal expansion coefficient28.3–29.7µstrain/°C
Thermal shock resistance391–533°C
Thermal distortion resistance0.016–0.0169MW/m

PARA 20% Glass Fiber Wear Grade Electrical properties

Electrical resistivity2e20–5e21µohm.cm
Electrical conductivity3.45e-20–8.62e-19%IACS
Dielectric constant (relative permittivity)3.45–4.86 
Dissipation factor (dielectric loss tangent)0.0181–0.0476 
Dielectric strength (dielectric breakdown)20.8–35.4MV/m
Comparative tracking index600  V

PARA 20% Glass Fiber Wear Grade Magnetic properties

Magnetic typeNon-magnetic

PARA 20% Glass Fiber Wear Grade Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity2180–2440m/s
Mechanical loss coefficient (tan delta)0.00984–0.0109 

PARA 20% Glass Fiber Wear Grade Absorption & permeability

Water absorption @ 24 hrs0.17–0.27%
Water absorption @ sat4–5.3%
Humidity absorption @ sat1.5–2.1%

PARA 20% Glass Fiber Wear Grade Processing properties

Polymer injection moldingLimited use
Polymer extrusionAcceptable
Polymer thermoformingLimited use
Linear mold shrinkage0.2 – 0.4 %
Melt temperature269 – 291 °C
Mold temperature122 – 138 °C
Molding pressure range30 – 150 MPa

PARA 20% Glass Fiber Wear Grade Durability

Water (fresh)Excellent
Water (salt)Acceptable
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsLimited use
Oils and fuelsAcceptable
Oxidation at 500CUnacceptable
UV radiation (sunlight)Good
FlammabilitySlow-burning