PARA 50% Glass Fiber Toughened Material Data Sheet

PARA 50% Glass Fiber Toughened (Polyarylamide) Material Data Sheet

PARA 50% Glass Fiber Toughened Overview

PARA 50% glass fiber toughened is a grade of polyarylamide (PARA), designated Polyarylamide (50% glass fiber, toughened). This PARA 50% glass fiber toughened material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PARA parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PARA parts in-house and inspects them before shipment.

PARA 50% Glass Fiber Toughened Designation

Polyarylamide (50% glass fiber, toughened)
TradenamesIxef

PARA 50% Glass Fiber Toughened Typical uses

Automotive, furniture, small appliances, lawn mowers, power tools, electrical contactors and switches, electrical motor components, cell phones, faucet components.

PARA 50% Glass Fiber Toughened Composition detail

Polymer35–45%
Impact modifier5–15%
Glass (fiber)50  %

PARA 50% Glass Fiber Toughened Physical properties

Density1.62–1.65g/cm3

PARA 50% Glass Fiber Toughened Mechanical properties

Young’s modulus14.2–17.8GPa
Specific stiffness8.68–10.9MN.m/kg
Yield strength (elastic limit)178–222MPa
Tensile strength180–220MPa
Specific strength109–136kN.m/kg
Elongation2.21–3.19% strain
Elongation at yield1.86–3.54% strain
Compressive modulus15.2–16.8GPa
Compressive strength228–252MPa
Flexural modulus14.5–17.4GPa
Flexural strength (modulus of rupture)270–329MPa
Shear modulus5.83–6.13GPa
Shear strength108–132MPa
Bulk modulus15.5–17.2GPa
Poisson’s ratio0.335–0.337 
Shape factor7.1
Hardness – Vickers57–63HV
Hardness – Rockwell M184–204 
Hardness – Rockwell R184–204 
Hardness – Shore D98–102 
Elastic stored energy (springs)984–1570kJ/m3
Fatigue strength at 10^7 cycles76–84MPa

PARA 50% Glass Fiber Toughened Impact & fracture properties

Fracture toughness5.36–5.92MPa.m0.5
Toughness (G)1.72–2.31kJ/m2
Impact strength, notched 23 °C8.64–16.8kJ/m2
Impact strength, unnotched 23 °C66–97kJ/m2

PARA 50% Glass Fiber Toughened Thermal properties

Melting point259–281°C
Glass temperature78–92.2°C
Heat deflection temperature 0.45MPa237–258°C
Heat deflection temperature 1.8MPa210–230°C
Vicat softening point77–90°C
Maximum service temperature179–198°C
Thermal conductivity0.569–0.591W/m.°C
Specific heat capacity1240–1260J/kg.°C

PARA 50% Glass Fiber Toughened Electrical properties

Electrical resistivity2e20–5e21µohm.cm
Electrical conductivity3.45e-20–8.62e-19%IACS
Dielectric constant (relative permittivity)3.62–5.1 
Dissipation factor (dielectric loss tangent)0.0145–0.0381 
Dielectric strength (dielectric breakdown)18.5–31.5MV/m
Comparative tracking index400–450V

PARA 50% Glass Fiber Toughened Magnetic properties

Magnetic typeNon-magnetic

PARA 50% Glass Fiber Toughened Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity2940–3310m/s
Mechanical loss coefficient (tan delta)0.0063–0.00696 

PARA 50% Glass Fiber Toughened Absorption & permeability

Water absorption @ 24 hrs0.14–0.24%
Water absorption @ sat1.4–1.9%
Humidity absorption @ sat0.79–1.1%

PARA 50% Glass Fiber Toughened Processing properties

Polymer injection moldingLimited use
Polymer extrusionAcceptable
Polymer thermoformingLimited use
Linear mold shrinkage0.196 – 0.204 %
Melt temperature259 – 281 °C
Mold temperature122 – 138 °C
Molding pressure range30 – 150 MPa

PARA 50% Glass Fiber Toughened Durability

Water (fresh)Excellent
Water (salt)Acceptable
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsLimited use
Oils and fuelsAcceptable
Oxidation at 500CUnacceptable
UV radiation (sunlight)Good
FlammabilitySlow-burning