PA11 Rigid Grade Material Data Sheet

PA11 Rigid Grade (Polyamide 11) Material Data Sheet

PA11 Rigid Grade Overview

PA11 rigid grade is a grade of polyamide 11 (PA11, nylon 11), designated Polyamide (Nylon) (Type 11, rigid, molding and extrusion). This PA11 rigid grade material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA11 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA11 parts in-house and inspects them before shipment.

PA11 Rigid Grade Designation

Polyamide (Nylon) (Type 11, rigid, molding and extrusion)
TradenamesAshlene, Hifill, Lubricomp, Rilsan

PA11 Rigid Grade Typical uses

Hose for air, hydraulic fluid or petrol, gears, cams, tool handles, powder for coatings for metals.

PA11 Rigid Grade Composition detail

Polymer100  %

PA11 Rigid Grade Physical properties

Density1.02–1.04g/cm3

PA11 Rigid Grade Mechanical properties

Young’s modulus1.06–1.33GPa
Specific stiffness1.03–1.29MN.m/kg
Yield strength (elastic limit)35.4–44.1MPa
Tensile strength50–55MPa
Specific strength34.4–42.8kN.m/kg
Elongation280–320% strain
Elongation at yield8–15% strain
Compressive modulus1.14–1.25GPa
Compressive strength60–66MPa
Flexural modulus1.09–1.3GPa
Flexural strength (modulus of rupture)56.9–69.6MPa
Shear modulus0.409–0.43GPa
Shear strength26.8–32.8MPa
Bulk modulus2.46–2.72GPa
Poisson’s ratio0.406–0.423 
Shape factor4.1
Hardness – Vickers11–13HV
Hardness – Rockwell M70–80 
Hardness – Rockwell R100–110 
Hardness – Shore D70–75 
Elastic stored energy (springs)521–829kJ/m3
Fatigue strength at 10^7 cycles20–22MPa

PA11 Rigid Grade Impact & fracture properties

Fracture toughness3.17–3.5MPa.m0.5
Toughness (G)8.07–10.8kJ/m2
Impact strength, notched 23 °C7.5–11kJ/m2
Impact strength, notched -30 °C2.1–2.7kJ/m2
Impact strength, unnotched 23 °C590–600kJ/m2
Impact strength, unnotched -30 °C590–600kJ/m2

PA11 Rigid Grade Thermal properties

Melting point180–190°C
Glass temperature36–48°C
Heat deflection temperature 0.45MPa129–170°C
Heat deflection temperature 1.8MPa40–52°C
Maximum service temperature80–110°C
Minimum service temperature-70–-55°C
Thermal conductivity0.19–0.29W/m.°C
Specific heat capacity1730–1770J/kg.°C
Thermal expansion coefficient176–184µstrain/°C
Thermal shock resistance158–216°C
Thermal distortion resistance0.00106–0.00161MW/m
Latent heat of fusion39  kJ/kg

PA11 Rigid Grade Electrical properties

Electrical resistivity2e19–5e20µohm.cm
Electrical conductivity3.45e-19–8.62e-18%IACS
Dielectric constant (relative permittivity)4.2–5.92 
Dissipation factor (dielectric loss tangent)0.0473–0.125 
Dielectric strength (dielectric breakdown)25–35MV/m
Comparative tracking index600  V

PA11 Rigid Grade Magnetic properties

Magnetic typeNon-magnetic

PA11 Rigid Grade Optical, aesthetic and acoustic properties

Refractive index1.51–1.53 
TransparencyTranslucent
Acoustic velocity1010–1140m/s
Mechanical loss coefficient (tan delta)0.023–0.0254 

PA11 Rigid Grade Absorption & permeability

Water absorption @ 24 hrs0.68–1.1%
Water absorption @ sat1.6–2.2%
Humidity absorption @ sat0.68–0.92%
Water vapor transmission0.41  g.mm/m².day
Permeability (O2)17  cm³.mm/m².day.atm

PA11 Rigid Grade Processing properties

Polymer injection moldingExcellent
Polymer extrusionAcceptable
Polymer thermoformingLimited use
Linear mold shrinkage1 – 2 %
Melt temperature199 – 246 °C
Mold temperature40 – 60 °C
Molding pressure range16 – 70 MPa

PA11 Rigid Grade Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisLimited use
Organic solventsAcceptable
Oils and fuelsAcceptable
Oxidation at 500CUnacceptable
UV radiation (sunlight)Fair
FlammabilitySlow-burning

PA11 Rigid Grade Notes

PA11 Rigid Grade Other notes
PA type 11 is not petroleum-based, but uses C11 derivatives of castor oil (a vegetable oil extracted from castor seeds) as its main chemical feedstock.