PA46 30% Glass Fiber (Polyamide 46) Material Data Sheet
PA46 30% Glass Fiber Overview
PA46 30% glass fiber is a grade of polyamide 46 (PA46, nylon 46), designated Polyamide (Nylon) (Type 46, 30% Glass Fiber). This PA46 30% glass fiber material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA46 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA46 parts in-house and inspects them before shipment.
PA46 30% Glass Fiber Designation
Polyamide (Nylon) (Type 46, 30% Glass Fiber)
Tradenames
Alcom, Hifill, Pentamid, Stanyl
PA46 30% Glass Fiber Typical uses
Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.
PA46 30% Glass Fiber Composition detail
Polymer
70
%
Glass (fiber)
30
%
PA46 30% Glass Fiber Physical properties
Density
1.42
–
1.45
g/cm3
PA46 30% Glass Fiber Mechanical properties
Young’s modulus
5.34
–
6.66
GPa
Specific stiffness
3.72
–
4.64
MN.m/kg
Yield strength (elastic limit)
102
–
127
MPa
Tensile strength
103
–
126
MPa
Specific strength
71.1
–
88.5
kN.m/kg
Elongation
5.51
–
7.92
% strain
Elongation at yield
4.63
–
8.8
% strain
Compressive modulus
5.7
–
6.3
GPa
Compressive strength
130
–
144
MPa
Flexural modulus
5.05
–
6.05
GPa
Flexural strength (modulus of rupture)
162
–
198
MPa
Shear modulus
2.14
–
2.25
GPa
Shear strength
61.7
–
75.4
MPa
Bulk modulus
7.04
–
7.78
GPa
Poisson’s ratio
0.351
–
0.365
Shape factor
5.4
Hardness – Vickers
33
–
36
HV
Hardness – Rockwell M
155
–
171
Hardness – Rockwell R
155
–
171
Hardness – Shore D
91
–
95
Elastic stored energy (springs)
862
–
1370
kJ/m3
Fatigue strength at 10^7 cycles
43.4
–
48
MPa
PA46 30% Glass Fiber Impact & fracture properties
Fracture toughness
4.39
–
4.86
MPa.m0.5
Toughness (G)
3.09
–
4.14
kJ/m2
Impact strength, notched 23 °C
12.8
–
24.9
kJ/m2
Impact strength, notched -30 °C
6.93
–
15.1
kJ/m2
Impact strength, unnotched 23 °C
77.5
–
114
kJ/m2
Impact strength, unnotched -30 °C
55.4
–
83.1
kJ/m2
PA46 30% Glass Fiber Thermal properties
Melting point
284
–
306
°C
Glass temperature
71
–
79
°C
Heat deflection temperature 0.45MPa
284
–
340
°C
Heat deflection temperature 1.8MPa
258
–
313
°C
Maximum service temperature
73
–
87
°C
Minimum service temperature
-58
–
-38
°C
Thermal conductivity
0.447
–
0.464
W/m.°C
Specific heat capacity
1370
–
1430
J/kg.°C
Thermal expansion coefficient
46.8
–
47.8
µstrain/°C
Thermal shock resistance
346
–
470
°C
Thermal distortion resistance
0.00942
–
0.00984
MW/m
PA46 30% Glass Fiber Electrical properties
Electrical resistivity
8.12e15
–
2.03e17
µohm.cm
Electrical conductivity
8.49e-16
–
2.12e-14
%IACS
Dielectric constant (relative permittivity)
12.2
–
17.2
Dissipation factor (dielectric loss tangent)
0.248
–
0.653
Dielectric strength (dielectric breakdown)
16.7
–
28.4
MV/m
Comparative tracking index
375
–
425
V
PA46 30% Glass Fiber Magnetic properties
Magnetic type
Non-magnetic
PA46 30% Glass Fiber Optical, aesthetic and acoustic properties