PA46 50% Glass Fiber Material Data Sheet

PA46 50% Glass Fiber (Polyamide 46) Material Data Sheet

PA46 50% Glass Fiber Overview

PA46 50% glass fiber is a grade of polyamide 46 (PA46, nylon 46), designated Polyamide (Nylon) (Type 46, 50% Glass Fiber). This PA46 50% glass fiber material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA46 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA46 parts in-house and inspects them before shipment.

PA46 50% Glass Fiber Designation

Polyamide (Nylon) (Type 46, 50% Glass Fiber)
TradenamesHifill, Stanyl, Stanyl Diablo

PA46 50% Glass Fiber Typical uses

Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.

PA46 50% Glass Fiber Composition detail

Polymer50  %
Glass (fiber)50  %

PA46 50% Glass Fiber Physical properties

Density1.62–1.65g/cm3

PA46 50% Glass Fiber Mechanical properties

Young’s modulus8.9–11.1GPa
Specific stiffness5.44–6.79MN.m/kg
Yield strength (elastic limit)142–178MPa
Tensile strength144–176MPa
Specific strength86.8–109kN.m/kg
Elongation4.1–5.9% strain
Elongation at yield3.45–6.55% strain
Compressive modulus9.5–10.5GPa
Compressive strength182–202MPa
Flexural modulus8.19–9.81GPa
Flexural strength (modulus of rupture)225–275MPa
Shear modulus3.63–3.82GPa
Shear strength86.4–106MPa
Bulk modulus10.1–11.1GPa
Poisson’s ratio0.329–0.343 
Shape factor6
Hardness – Vickers46–50HV
Hardness – Rockwell M181–200 
Hardness – Rockwell R181–200 
Hardness – Shore D97–101 
Elastic stored energy (springs)1000–1610kJ/m3
Fatigue strength at 10^7 cycles60.8–67.2MPa

PA46 50% Glass Fiber Impact & fracture properties

Fracture toughness4.87–5.38MPa.m0.5
Toughness (G)2.28–3.04kJ/m2
Impact strength, notched 23 °C16.3–31.7kJ/m2
Impact strength, notched -30 °C8.82–19.2kJ/m2
Impact strength, unnotched 23 °C89.1–131kJ/m2
Impact strength, unnotched -30 °C80–120kJ/m2

PA46 50% Glass Fiber Thermal properties

Melting point284–306°C
Glass temperature71–79°C
Heat deflection temperature 0.45MPa284–340°C
Heat deflection temperature 1.8MPa258–313°C
Maximum service temperature73–87°C
Minimum service temperature-58–-38°C
Thermal conductivity0.597–0.621W/m.°C
Specific heat capacity1240–1290J/kg.°C
Thermal expansion coefficient27.5–28.1µstrain/°C
Thermal shock resistance493–672°C
Thermal distortion resistance0.0214–0.0224MW/m

PA46 50% Glass Fiber Electrical properties

Electrical resistivity2e15–5e16µohm.cm
Electrical conductivity3.45e-15–8.62e-14%IACS
Dielectric constant (relative permittivity)13.3–18.7 
Dissipation factor (dielectric loss tangent)0.33–0.87 
Dielectric strength (dielectric breakdown)14.8–25.2MV/m
Comparative tracking index325–375V

PA46 50% Glass Fiber Magnetic properties

Magnetic typeNon-magnetic

PA46 50% Glass Fiber Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity2330–2610m/s
Mechanical loss coefficient (tan delta)0.00838–0.00926 

PA46 50% Glass Fiber Absorption & permeability

Water absorption @ 24 hrs1.4–2.4%
Water absorption @ sat5.8–7.7%
Humidity absorption @ sat1.6–2.1%

PA46 50% Glass Fiber Processing properties

Polymer injection moldingAcceptable
Polymer extrusionAcceptable
Polymer thermoformingLimited use
Linear mold shrinkage0.2 – 0.4 %
Melt temperature242 – 316 °C
Mold temperature40 – 80 °C
Molding pressure range34.4 – 103 MPa

PA46 50% Glass Fiber Durability

Water (fresh)Acceptable
Water (salt)Acceptable
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisUnacceptable
Organic solventsAcceptable
Oxidation at 500CUnacceptable
UV radiation (sunlight)Fair
FlammabilitySlow-burning