PA6 Cast Grade (Polyamide 6) Material Data Sheet
PA6 Cast Grade Overview
| PA6 cast grade is a grade of polyamide 6 (PA6, nylon 6), designated Polyamide (Nylon) (Type 6, Cast). This PA6 cast grade material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA6 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined cast PA6 parts in-house and inspects them before shipment. |
PA6 Cast Grade Designation
| Polyamide (Nylon) (Type 6, Cast) | |
| Tradenames | 4Mid, Addinyl, Aegis, Akromid, Akulon, Akulon Ultraflow, Alcom, Alphalon, Altech, Amilan, Anjacom, Anjamid, Aquamid, Armamid, Ashlene, Astamid, Badamid, Bergamid, Bestnyl, Capran, Capran Medallion, Chemlon, Clariant, Comco, Compamid, Denyl, Deslon, Dinalon, Distrumid, Domamid, Durethan, Dynacom, Ecotan, Eplamid, Germamid, Glamide, Gravi-Tech, Grilon, Heramid, Hifill, Hylon, Hylonselect, Isocor, Kepamid, Kopa, Lamigamid, LNP Thermocomp, Lumid, Luvocom, Mazmid, Miramid, Next Industrial, Next Prime, Nilamid, Niretan, Novamid, Novamide, Nybex, Nycal, Nycast, Nylaforce, Nylamid, Nylene, Nylfor, Nymax, Nypol, Nyrim, Orgalloy, Pentamid, Plustek, Polybest, Promyde, Pryme, Quadrant, Radici, Radilon, Scanamid, Schulamid, Selar, Shokamid, Silamid, Slovamid, Staramide, Tarnamid, Taromid, Technamid, Technyl, Technyl Star, Tekamid, Tekumid, Terez, Thermocomp, Thermylon, Tufnyl, Ultramid, Unitika, Venyl, Vitamide, Wellamid, Zytel |
PA6 Cast Grade Typical uses
| Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils. |
PA6 Cast Grade Composition detail
| Polymer | 100 | % |
PA6 Cast Grade Physical properties
| Density | 1.14 | – | 1.16 | g/cm3 |
PA6 Cast Grade Mechanical properties
| Young’s modulus | 1.58 | – | 1.97 | GPa |
| Specific stiffness | 1.37 | – | 1.71 | MN.m/kg |
| Yield strength (elastic limit) | 51.2 | – | 63.8 | MPa |
| Tensile strength | 64.7 | – | 79.1 | MPa |
| Specific strength | 44.5 | – | 55.5 | kN.m/kg |
| Elongation | 61.5 | – | 88.5 | % strain |
| Elongation at yield | 5.58 | – | 10.6 | % strain |
| Compressive modulus | 1.69 | – | 1.86 | GPa |
| Compressive strength | 81.9 | – | 90.6 | MPa |
| Flexural modulus | 1.62 | – | 1.93 | GPa |
| Flexural strength (modulus of rupture) | 54 | – | 66 | MPa |
| Shear modulus | 0.636 | – | 0.669 | GPa |
| Shear strength | 38.8 | – | 47.4 | MPa |
| Bulk modulus | 2.01 | – | 2.22 | GPa |
| Poisson’s ratio | 0.34 | – | 0.36 | |
| Shape factor | 4.2 | |||
| Hardness – Vickers | 16 | – | 18 | HV |
| Hardness – Rockwell M | 122 | – | 135 | |
| Hardness – Rockwell R | 122 | – | 135 | |
| Hardness – Brinell | 111 | – | 139 | HB |
| Hardness – Shore D | 87 | – | 93 | |
| Elastic stored energy (springs) | 735 | – | 1170 | kJ/m3 |
| Fatigue strength at 10^7 cycles | 27.3 | – | 30.2 | MPa |
PA6 Cast Grade Impact & fracture properties
| Fracture toughness | 3.43 | – | 3.8 | MPa.m0.5 |
| Toughness (G) | 6.39 | – | 8.55 | kJ/m2 |
| Impact strength, notched 23 °C | 10.2 | – | 19.8 | kJ/m2 |
PA6 Cast Grade Thermal properties
| Melting point | 227 | – | 238 | °C |
| Glass temperature | 44 | – | 56 | °C |
| Heat deflection temperature 0.45MPa | 204 | – | 221 | °C |
| Heat deflection temperature 1.8MPa | 166 | – | 204 | °C |
| Maximum service temperature | 90 | – | 130 | °C |
| Minimum service temperature | -64 | – | -54 | °C |
| Thermal conductivity | 0.294 | – | 0.306 | W/m.°C |
| Specific heat capacity | 1400 | – | 1500 | J/kg.°C |
| Thermal expansion coefficient | 88.2 | – | 91.8 | µstrain/°C |
| Thermal shock resistance | 309 | – | 420 | °C |
| Thermal distortion resistance | 0.00324 | – | 0.00343 | MW/m |
PA6 Cast Grade Electrical properties
| Electrical resistivity | 2e17 | – | 5e18 | µohm.cm |
| Electrical conductivity | 3.45e-17 | – | 8.62e-16 | %IACS |
| Dielectric constant (relative permittivity) | 5.48 | – | 7.72 | |
| Dissipation factor (dielectric loss tangent) | 0.077 | – | 0.203 | |
| Dielectric strength (dielectric breakdown) | 13.7 | – | 23.3 | MV/m |
| Comparative tracking index | 600 | V |
PA6 Cast Grade Magnetic properties
| Magnetic type | Non-magnetic |
PA6 Cast Grade Optical, aesthetic and acoustic properties
| Refractive index | 1.56 | – | 1.57 | |
| Transparency | Translucent | |||
| Acoustic velocity | 1170 | – | 1310 | m/s |
| Mechanical loss coefficient (tan delta) | 0.0189 | – | 0.0209 | |
PA6 Cast Grade Absorption & permeability
| Water absorption @ 24 hrs | 0.8 | – | 1.3 | % |
| Water absorption @ sat | 5.2 | – | 6.8 | % |
| Humidity absorption @ sat | 1.9 | – | 2.5 | % |
| Water vapor transmission | 0.958 | – | 1.73 | g.mm/m².day |
| Permeability (O2) | 0.622 | – | 1.15 | cm³.mm/m².day.atm |
PA6 Cast Grade Processing properties
| Polymer injection molding | Unsuitable |
| Polymer extrusion | Unsuitable |
| Polymer thermoforming | Unsuitable |
| Linear mold shrinkage | 0.1 – 1 % |
PA6 Cast Grade Durability
| Water (fresh) | Excellent |
| Water (salt) | Acceptable |
| Weak acids | Unacceptable |
| Strong acids | Unacceptable |
| Weak alkalis | Limited use |
| Strong alkalis | Limited use |
| Organic solvents | Acceptable |
| Oxidation at 500C | Unacceptable |
| UV radiation (sunlight) | Fair |
| Flammability | Slow-burning |