Modified PEEK 25-30% Carbon Wear Grade Material Data Sheet

Modified PEEK 25-30% Carbon Wear Grade (Polyetheretherketone) Material Data Sheet

Modified PEEK 25-30% Carbon Wear Grade Overview

Modified PEEK 25-30% carbon wear grade is a grade of polyetheretherketone (PEEK), designated Modified poly(etheretherketone) (Wear grade). This modified PEEK 25-30% carbon wear grade material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PEEK parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PEEK parts in-house and inspects them before shipment.

Modified PEEK Designation

Modified poly(etheretherketone) (Wear grade)
TradenamesAvaSpire

Modified PEEK 25-30% Carbon Wear Grade Composition detail

Polymer65–75%
PTFE (lubricant)0–10%
Carbon (fiber)15–25%
Graphite (powder)0–10%

Modified PEEK Physical properties

Density1.45–1.48g/cm3

Modified PEEK 25-30% Carbon Wear Grade Mechanical properties

Young’s modulus12.3–13.1GPa
Specific stiffness8.37–8.97MN.m/kg
Yield strength (elastic limit)111–118MPa
Tensile strength135–144MPa
Specific strength75.7–80.7kN.m/kg
Elongation1.74–2.16% strain
Elongation at yield1.7–2.1% strain
Compressive modulus12.3–13.1GPa
Flexural modulus12.3–13.1GPa
Flexural strength (modulus of rupture)211–213MPa
Shear modulus4.6–4.9GPa
Shear strength67.5–74.5MPa
Poisson’s ratio0.42–0.46 
Shape factor8.8
Hardness – Vickers33–35HV
Elastic stored energy (springs)482–552kJ/m3
Fatigue strength at 10^7 cycles53–58.6MPa

Modified PEEK Impact & fracture properties

Impact strength, notched 23 °C4.97–7.23kJ/m2
Impact strength, unnotched 23 °C40.2–45.8kJ/m2

Modified PEEK 25-30% Carbon Wear Grade Thermal properties

Melting point613–616°C
Glass temperature150–168°C
Heat deflection temperature 0.45MPa554–563°C
Heat deflection temperature 1.8MPa540–549°C
Vicat softening point554–563°C
Thermal conductivity0.3–0.34W/m.°C
Specific heat capacity1350–1380J/kg.°C
Thermal expansion coefficient9.88–10.1µstrain/°C
Thermal shock resistance862–945°C
Thermal distortion resistance0.03–0.0341MW/m

Modified PEEK Electrical properties

Electrical resistivity25000000000000000–100000000000000000µohm.cm
Electrical conductivity1.72e-15–6.9e-15%IACS
Dielectric constant (relative permittivity)3.3–4 
Dissipation factor (dielectric loss tangent)0.001–0.006 
Dielectric strength (dielectric breakdown)30–70MV/m
Galvanic potential0.14–0.22V

Modified PEEK Magnetic properties

Magnetic typeNon-magnetic

Modified PEEK Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity2890–3000m/s

Modified PEEK Processing properties

Polymer injection moldingLimited use
Polymer extrusionAcceptable
Polymer thermoformingUnsuitable
Melt temperature366 – 388 °C
Mold temperature149 – 177 °C

Modified PEEK Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsExcellent
Strong acidsLimited use
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oils and fuelsExcellent
Oxidation at 500CUnacceptable
UV radiation (sunlight)Excellent
FlammabilitySelf-extinguishing