Cu-Cd-Sn H.C. Copper, Soft Material Data Sheet

Cu-Cd-Sn H.C. Copper Material Data Sheet (Wrought, Soft)

Cu-Cd-Sn Soft Copper Overview

Cu-Cd-Sn soft copper is a wrought high conductivity copper, known as h.c. copper. Condition: Soft. This Cu-Cd-Sn soft copper material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for Cu-Cd-Sn copper parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined Cu-Cd-Sn copper parts in-house and inspects them before shipment.

Cu-Cd-Sn Designation

Wrought Copper Alloy: hc-CuCd1Sn(s)
ConditionSoft
UNS numberC16400, C16500

Cu-Cd-Sn Typical uses

Catenary trolley wires, telephone wires, spring contacts, flexible cords, plugs & sockets, overhead lines.

Cu-Cd-Sn Soft Copper Composition detail

Cd (cadmium)0.5–1%
Cu (copper)98.4–99.3%
Sn (tin)0.2–0.6%

Cu-Cd-Sn Physical properties

Density8.94–8.95g/cm3

Cu-Cd-Sn Soft Copper Mechanical properties

Young’s modulus133–135GPa
Specific stiffness14.9–15.1MN.m/kg
Yield strength (elastic limit)85–95MPa
Tensile strength250–280MPa
Specific strength9.51–10.6kN.m/kg
Elongation40–45% strain
Compressive strength85–95MPa
Flexural modulus133–135GPa
Flexural strength (modulus of rupture)85–95MPa
Shear modulus48–50GPa
Bulk modulus144–146GPa
Poisson’s ratio0.34–0.35 
Shape factor30
Hardness – Vickers57–59HV
Elastic stored energy (springs)27–33.6kJ/m3
Fatigue strength at 10^7 cycles130–140MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
120–152MPa

Cu-Cd-Sn Impact & fracture properties

Fracture toughness77.6–80.9MPa.m0.5
Toughness (G)44.9–48.9kJ/m2

Cu-Cd-Sn Soft Copper Thermal properties

Melting point1010–1080°C
Maximum service temperature77–87°C
Minimum service temperature-273  °C
Thermal conductivity207–248W/m.°C
Specific heat capacity372–385J/kg.°C
Thermal expansion coefficient17–17.5µstrain/°C
Thermal shock resistance36.7–41.2°C
Thermal distortion resistance12–14.4MW/m
Latent heat of fusion200–208kJ/kg

Cu-Cd-Sn Electrical properties

Electrical resistivity2.29–2.88µohm.cm
Electrical conductivity59.9–75.3%IACS
Temperature dependence of resistivity5.2–5.4/°C
Galvanic potential-0.21–-0.13V

Cu-Cd-Sn Magnetic properties

Magnetic typeNon-magnetic

Cu-Cd-Sn Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3860–3890m/s
Mechanical loss coefficient (tan delta)4.43e-4–5.54e-4 

Cu-Cd-Sn Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingAcceptable
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed29 m/min
Weldability
Notes: Preheating and post weld heat treatment are not required, and contains hazardous elements
Good

Cu-Cd-Sn Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

Cu-Cd-Sn Soft Copper Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Not susceptible

Cu-Cd-Sn Notes

Cu-Cd-Sn Soft Copper Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

Cu-Cd-Sn Standards with similar compositions

Germany: 2.127 to DIN, CuCdSn to DIN
USA: C16500, UNS C16400, UNS C16500
Tradenames: HITENSO 165, PHONO CADMIUM 955