Home » High Conductivity Copper » C18100 H.C. Copper, Solution Treated & Aged Material Data Sheet
C18100 H.C. Copper Material Data Sheet (Wrought, Solution Treated & Aged)
C18100 Solution Treated Aged Copper Overview
C18100 solution treated aged copper is a wrought high conductivity copper (UNS C18100, EN CW106C), known as h.c. copper. Condition: Solution heat-treated & precipitation hardened. This C18100 solution treated aged copper material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C18100 copper parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C18100 copper parts in-house and inspects them before shipment.
C18100 Designation
Copper Alloy: hc-CuCr1Zr(wp) (UNS C18100) Condition Solution heat-treated & precipitation hardened UNS number C18100 EN name CW106C ISO name CuCr1Zr
C18100 Solution Treated Aged Copper Composition detail
Cr (chromium) 0.4 – 1 % Cu (copper) 98.7 – 99.5 % Mg (magnesium) 0.03 – 0.06 % Zr (zirconium) 0.08 – 0.2 %
C18100 Physical properties
C18100 Solution Treated Aged Copper Mechanical properties
Young’s modulus 122 – 128 GPa Specific stiffness 13.6 – 14.3 MN.m/kg Yield strength (elastic limit) 240 – 255 MPa Tensile strength 355 – 375 MPa Specific strength 26.8 – 28.5 kN.m/kg Elongation 24 – 25.5 % strain Compressive strength 240 – 255 MPa Flexural modulus 122 – 128 GPa Flexural strength (modulus of rupture) 240 – 255 MPa Shear modulus 45.1 – 47.4 GPa Bulk modulus 132 – 138 GPa Poisson’s ratio 0.34 – 0.35 Shape factor 27 Hardness – Vickers 113 – 138 HV Elastic stored energy (springs) 230 – 261 kJ/m3 Fatigue strength at 10^7 cycles 100 – 110 MPa Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles 97.6 – 113 MPa
C18100 Impact & fracture properties
Fracture toughness 46.9 – 48.7 MPa.m0.5 Toughness (G) 17.5 – 19.1 kJ/m2
C18100 Solution Treated Aged Copper Thermal properties
Melting point 1080 °C Maximum service temperature 300 – 350 °C Minimum service temperature -273 °C Thermal conductivity 390 – 398 W/m.°C Specific heat capacity 383 – 387 J/kg.°C Thermal expansion coefficient 16.8 – 16.9 µstrain/°C Thermal shock resistance 113 – 122 °C Thermal distortion resistance 23.1 – 23.6 MW/m Latent heat of fusion 200 – 208 kJ/kg
C18100 Electrical properties
Electrical resistivity 2.09 – 2.19 µohm.cm Electrical conductivity 78.7 – 82.5 %IACS Temperature dependence of resistivity 5.2 – 5.4 /°C Galvanic potential -0.19 – -0.11 V
C18100 Magnetic properties
Magnetic type Non-magnetic
C18100 Optical, aesthetic and acoustic properties
Transparency Opaque Acoustic velocity 3690 – 3780 m/s Mechanical loss coefficient (tan delta) 6.2e-5 – 6.9e-5
C18100 Processing properties
Metal casting Unsuitable Metal cold forming Excellent Metal hot forming Excellent Metal press forming Excellent Metal deep drawing Limited use Machining speed 28.7 m/min Weldability Notes: Preheating and post weld heat treatment are not required Poor
C18100 Durability
Water (fresh) Excellent Water (salt) Excellent Weak acids Acceptable Strong acids Unacceptable Weak alkalis Excellent Strong alkalis Excellent Organic solvents Excellent Oxidation at 500C Limited use UV radiation (sunlight) Excellent Galling resistance (adhesive wear) Acceptable Flammability Non-flammable
C18100 Solution Treated Aged Copper Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide Not susceptible
C18100 Notes
C18100 Solution Treated Aged Copper Other notes (s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
C18100 Standards with similar compositions
Europe: CW106C to CEN EN 12163, CW106C to CEN EN 12165, CW106C to CEN EN 12167, CW106C to CEN EN 12420Germany: 2.1293 to DIN, CuCrZr to DINJapan: CuCr1Zr to JIS Z3234, CuCrZr to JIS Z3234USA: C18100, C18150, UNS C18100, UNS C18150Tradenames: AMPCOLOY 972, BOLTOMET 819, CERRO CCZ, CMW 328, ELBRODUR HF, WIELAND-K60
Modulus Metal Services