C16200 H.C. Copper, Soft Material Data Sheet

C16200 H.C. Copper Material Data Sheet (Wrought, Soft)

C16200 Soft Copper Overview

C16200 soft copper is a wrought high conductivity copper (UNS C16200, EN CW131C), known as h.c. copper. Condition: Soft. This C16200 soft copper material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C16200 copper parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C16200 copper parts in-house and inspects them before shipment.

C16200 Designation

Wrought Copper Alloy: hc-CuCd1(s); C108 (UNS C16200)
ConditionSoft
UNS numberC16200
EN nameCW131C
ISO nameCuCd1
GB (Chinese) nameQCd1

C16200 Typical uses

Catenary trolley wires, telephone wires, spring contacts, flexible cords, plugs & sockets, overhead lines.

C16200 Soft Copper Composition detail

Cd (cadmium)0.7–1.2%
Cu (copper)98.8–99.3%
Fe (iron)0–0.02%

C16200 Physical properties

Density8.94–8.95g/cm3

C16200 Soft Copper Mechanical properties

Young’s modulus133–135GPa
Specific stiffness14.9–15.1MN.m/kg
Yield strength (elastic limit)80–90MPa
Tensile strength250–270MPa
Specific strength8.95–10.1kN.m/kg
Elongation40–45% strain
Compressive strength80–90MPa
Flexural modulus133–135GPa
Flexural strength (modulus of rupture)80–90MPa
Shear modulus48–50GPa
Bulk modulus144–146GPa
Poisson’s ratio0.34–0.35 
Shape factor30
Hardness – Vickers58–60HV
Elastic stored energy (springs)24–30.1kJ/m3
Fatigue strength at 10^7 cycles90–110MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
87.8–113MPa

C16200 Impact & fracture properties

Fracture toughness79.2–82.6MPa.m0.5
Toughness (G)46.8–50.9kJ/m2

C16200 Soft Copper Thermal properties

Melting point1010–1080°C
Maximum service temperature77–87°C
Minimum service temperature-273  °C
Thermal conductivity310–351W/m.°C
Specific heat capacity372–385J/kg.°C
Thermal expansion coefficient16.8–16.9µstrain/°C
Thermal shock resistance35.4–39.9°C
Thermal distortion resistance18.4–20.8MW/m
Latent heat of fusion200–208kJ/kg

C16200 Electrical properties

Electrical resistivity1.91–2.19µohm.cm
Electrical conductivity78.7–90.3%IACS
Temperature dependence of resistivity5.2–5.4/°C
Galvanic potential-0.2–-0.12V

C16200 Magnetic properties

Magnetic typeNon-magnetic

C16200 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3860–3890m/s
Mechanical loss coefficient (tan delta)4.94e-4–6.25e-4 

C16200 Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingAcceptable
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed29.6 m/min
Weldability
Notes: Preheating and post weld heat treatment are not required, and contains hazardous elements
Good

C16200 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

C16200 Soft Copper Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Not susceptible

C16200 Notes

C16200 Soft Copper Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

C16200 Standards with similar compositions

Australia: 162 to AS 1567, C16200 to AS 2738
Czech Republic: CuCd1 to CSN 423058
Germany: 2.1266 to DIN, CuCd1 to DIN
International: CuCd1 to ISO 1637, CuCd1 to ISO 1638, CuCd1 to ISO R1336
Japan: CuCd1 to JIS Z3234
Sweden: 5055-25 to SIS 145055
UK: C108 to BS 2873, C108 to BS 2875
USA: C16200, UNS C16200, UNS C16210
Tradenames: ANSONIA ALLOY C 16200, BOLTOMET 210, BRIDGEPORT NO. 980, BRIDGEPORT NO. 985, BRONZE AU-CADMIUM, CADMIUM COPPER, CADMIUM COPPER 985, ELECTRAL CD 1, HITENSO 162, HI-TENSO 1622, LITHIUM-CONDUCTIVITY BRONZE, PHONO HI CONDUCTIVITY, PHONO HI-CONDUCTIVITY 985, TRIANGLE 80, TRIANGLE 85