C15100 H.C. Copper, Solution Treated & Aged Material Data Sheet

C15100 H.C. Copper Material Data Sheet (Wrought, Solution Treated & Aged)

C15100 Solution Treated Aged Copper Overview

C15100 solution treated aged copper is a wrought high conductivity copper (UNS C15100, EN CW120C), known as h.c. copper. Condition: Solution heat-treated & precipitation hardened. This C15100 solution treated aged copper material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C15100 copper parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C15100 copper parts in-house and inspects them before shipment.

C15100 Designation

Copper Alloy: hc-CuZr(wp) (UNS C15100)
ConditionSolution heat-treated & precipitation hardened
UNS numberC15100
EN nameCW120C
ISO nameCuZr
JIS (Japanese) nameC1500

C15100 Solution Treated Aged Copper Composition detail

Al (aluminum)0–0.005%
Cu (copper)99.8–100%
Fe (iron)0–0.005%
Mn (manganese)0–0.005%
Zr (zirconium)0.05–0.15%

C15100 Physical properties

Density8.94–8.95g/cm3

C15100 Solution Treated Aged Copper Mechanical properties

Young’s modulus122–128GPa
Specific stiffness13.6–14.3MN.m/kg
Yield strength (elastic limit)220–230MPa
Tensile strength300–320MPa
Specific strength24.6–25.7kN.m/kg
Elongation34–36% strain
Compressive strength220–230MPa
Flexural modulus122–128GPa
Flexural strength (modulus of rupture)220–230MPa
Shear modulus45.1–47.4GPa
Bulk modulus132–138GPa
Poisson’s ratio0.34–0.35 
Shape factor28
Hardness – Vickers115–125HV
Elastic stored energy (springs)193–213kJ/m3
Fatigue strength at 10^7 cycles90–100MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
87.4–103MPa

C15100 Impact & fracture properties

Fracture toughness50–51.4MPa.m0.5
Toughness (G)19.8–21.3kJ/m2

C15100 Solution Treated Aged Copper Thermal properties

Melting point1080  °C
Maximum service temperature300–350°C
Minimum service temperature-273  °C
Thermal conductivity390–398W/m.°C
Specific heat capacity383–387J/kg.°C
Thermal expansion coefficient16.8–16.9µstrain/°C
Thermal shock resistance103–110°C
Thermal distortion resistance23.1–23.6MW/m
Latent heat of fusion200–208kJ/kg

C15100 Electrical properties

Electrical resistivity1.91–2.04µohm.cm
Electrical conductivity84.5–90.3%IACS
Temperature dependence of resistivity5.2–5.4/°C
Galvanic potential-0.2–-0.12V

C15100 Magnetic properties

Magnetic typeNon-magnetic

C15100 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3690–3780m/s
Mechanical loss coefficient (tan delta)7.6e-5–8.3e-5 

C15100 Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed29 m/min
Weldability
Notes: Preheating and post weld heat treatment are not required
Poor

C15100 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

C15100 Solution Treated Aged Copper Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Not susceptible

C15100 Notes

C15100 Solution Treated Aged Copper Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

C15100 Standards with similar compositions

Europe: CW120C to CEN EN 12163, CW120C to CEN EN 12165, CW120C to CEN EN 12166, CW120C to CEN EN 12167, CW120C to CEN EN 12420
Germany: 2.158 to DIN, CuZr to DIN
Japan: CuZr to JIS Z3234
USA: C15000, C15000 to SAE J463, C15100, C15100 to ASTM B747, C15100 to ASTM B888, UNS C15000, UNS C15100
Tradenames: AMPCO 910, AMPCOLOY 910, AMZIRC-150, ANSONIA ALLOY C15000, BRIDGEPORT NO. 992, CMW 28, ELBRODUR N4, ELECTRAL CRM 16N, MITSUBISHI MKZ, OLIN C151, OUTOKUMPU ZRK015, PMX ALLOY C15100 (PMX 151), REVERE ZIRCONIUM COPPER, ZIRCONIUM COPPER, ZIRCONIUM COPPER 150, ZIRCONIUM-COPPER 992, ZIRCONIUM-COPPER N-4 (NIPPERT ALLOY N-4)