C14500 H.C. Copper, Soft Material Data Sheet

C14500 H.C. Copper Material Data Sheet (Wrought, Soft)

C14500 Soft Copper Overview

C14500 soft copper is a wrought high conductivity copper (UNS C14500), known as h.c. copper. Condition: Soft. This C14500 soft copper material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C14500 copper parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C14500 copper parts in-house and inspects them before shipment.

C14500 Designation

Wrought Copper Alloy: hc-CuTe(s); C109
ConditionSoft
UNS numberC14500

C14500 Soft Copper Composition detail

Cu (copper)99.3–99.6%
P (phosphorus)0.004–0.012%
Te (tellurium)0.4–0.7%

C14500 Physical properties

Density8.94–8.95g/cm3

C14500 Soft Copper Mechanical properties

Young’s modulus122–128GPa
Specific stiffness13.6–14.3MN.m/kg
Yield strength (elastic limit)55–65MPa
Tensile strength220–240MPa
Specific strength6.15–7.27kN.m/kg
Elongation38–42% strain
Compressive strength55–65MPa
Flexural modulus122–128GPa
Flexural strength (modulus of rupture)55–65MPa
Shear modulus44–46GPa
Bulk modulus132–138GPa
Poisson’s ratio0.34–0.35 
Shape factor30
Hardness – Vickers53–56HV
Elastic stored energy (springs)12.2–16.8kJ/m3
Fatigue strength at 10^7 cycles90–110MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
87.3–113MPa

C14500 Impact & fracture properties

Fracture toughness88.4–92.7MPa.m0.5
Toughness (G)62.2–69.1kJ/m2

C14500 Soft Copper Thermal properties

Melting point977–1080°C
Maximum service temperature77–87°C
Minimum service temperature-273  °C
Thermal conductivity365–376W/m.°C
Specific heat capacity375–385J/kg.°C
Thermal expansion coefficient16.8–16.9µstrain/°C
Thermal shock resistance26–31°C
Thermal distortion resistance21.7–22.3MW/m
Latent heat of fusion200–208kJ/kg

C14500 Electrical properties

Electrical resistivity1.74–1.82µohm.cm
Electrical conductivity94.7–99.1%IACS
Temperature dependence of resistivity5.2–5.4/°C
Galvanic potential-0.2–-0.12V

C14500 Magnetic properties

Magnetic typeNon-magnetic

C14500 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3690–3780m/s
Mechanical loss coefficient (tan delta)9.47e-4–0.00132 

C14500 Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed29 m/min
WeldabilityUnsuitable

C14500 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

C14500 Soft Copper Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Not susceptible

C14500 Notes

C14500 Soft Copper Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

C14500 Standards with similar compositions

Australia: 145 to AS 1567
Europe: CW118C to CEN EN 12164, CW118C to CEN EN 12166, CW118C to CEN EN 12168
International: CuTe to ISO 1637, CuTe to ISO R1336, CuTe(P) to ISO 1637, CuTe(P) to ISO R1336
UK: C109 to BS 2874
USA: C14500, C14500 to ASTM B124M, C14500 to ASTM B283, C14500 to ASTM B301/B301M, C14500 to SAE J463, C14510, C14510 to ASTM B301/B301M, C14520, C14520 to ASTM B301/B301M, UNS C14500, UNS C14510, UNS C14520
Tradenames: AMTEL, BRIDGEPORT NO. 112, CHASE TELLURIUM COPPER, ERM HSM, FUCHS 2050, IMI 180, KUTERN, MCKECHNIE TC, MITSUBISHI MKT, MUELLER 1450, NORANDA 1450, OSNA CU58TE, OUTOKUMPU TEK06, REVERE NO. 145, TELLURIUM COPPER, TELLURIUM COPPER 112, TELLURIUM COPPER 145