C10500 Silver-Bearing Oxygen-Free H.C. Copper Material Data Sheet (Wrought, Soft)
C10500 Soft Copper Overview
| C10500 soft copper is a wrought high conductivity copper (UNS C10500, EN CW017A), known as silver-bearing oxygen-free h.c. copper. Condition: Soft. This C10500 soft copper material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C10500 copper parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C10500 copper parts in-house and inspects them before shipment. |
C10500 Designation
| Wrought Copper Alloy: hc-Cu-OFS(s) (UNS C10500) | |
| Condition | Soft |
| UNS number | C10500 |
| EN name | CW017A |
| ISO name | CuAg0,05(OF) |
C10500 Typical uses
| Magnet windings for heavy-duty generators & motors, busbars, contacts, switches, glass to metal seals, transistor bases. |
C10500 Soft Copper Composition detail
| Ag (silver) | 0 | – | 0.02 | % |
| Cu (copper) | 99.9 | – | 100 | % |
C10500 Physical properties
| Density | 8.94 | – | 8.95 | g/cm3 |
C10500 Soft Copper Mechanical properties
| Young’s modulus | 120 | – | 125 | GPa |
| Specific stiffness | 13.4 | – | 14 | MN.m/kg |
| Yield strength (elastic limit) | 45 | – | 55 | MPa |
| Tensile strength | 210 | – | 230 | MPa |
| Specific strength | 5.03 | – | 6.15 | kN.m/kg |
| Elongation | 46 | – | 49 | % strain |
| Compressive strength | 45 | – | 55 | MPa |
| Flexural modulus | 120 | – | 125 | GPa |
| Flexural strength (modulus of rupture) | 45 | – | 55 | MPa |
| Shear modulus | 45 | – | 47 | GPa |
| Bulk modulus | 130 | – | 135 | GPa |
| Poisson’s ratio | 0.34 | – | 0.35 | |
| Shape factor | 30 | |||
| Hardness – Vickers | 45 | – | 55 | HV |
| Elastic stored energy (springs) | 8.34 | – | 12.2 | kJ/m3 |
| Fatigue strength at 10^7 cycles | 70 | – | 80 | MPa |
| Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles | 67 | – | 83.6 | MPa |
C10500 Impact & fracture properties
| Fracture toughness | 92.7 | – | 97.4 | MPa.m0.5 |
| Toughness (G) | 69.9 | – | 77.7 | kJ/m2 |
C10500 Soft Copper Thermal properties
| Melting point | 1080 | °C | ||
| Maximum service temperature | 77 | – | 87 | °C |
| Minimum service temperature | -273 | °C | ||
| Thermal conductivity | 387 | – | 392 | W/m.°C |
| Specific heat capacity | 378 | – | 385 | J/kg.°C |
| Thermal expansion coefficient | 16.8 | – | 16.9 | µstrain/°C |
| Thermal shock resistance | 21.8 | – | 26.7 | °C |
| Thermal distortion resistance | 23 | – | 23.3 | MW/m |
| Latent heat of fusion | 200 | – | 208 | kJ/kg |
C10500 Electrical properties
| Electrical resistivity | 1.7 | – | 1.74 | µohm.cm |
| Electrical conductivity | 99.1 | – | 101 | %IACS |
| Temperature dependence of resistivity | 5.2 | – | 5.4 | /°C |
| Galvanic potential | -0.2 | – | -0.12 | V |
C10500 Magnetic properties
| Magnetic type | Non-magnetic |
C10500 Optical, aesthetic and acoustic properties
| Transparency | Opaque | |||
| Acoustic velocity | 3660 | – | 3740 | m/s |
| Mechanical loss coefficient (tan delta) | 0.00132 | – | 0.00198 | |
C10500 Processing properties
| Metal casting | Unsuitable |
| Metal cold forming | Excellent |
| Metal hot forming | Excellent |
| Metal press forming | Excellent |
| Metal deep drawing | Limited use |
| Machining speed | 29 m/min |
| Weldability Notes: Preheating and post weld heat treatment are not required | Good |
C10500 Durability
| Water (fresh) | Excellent |
| Water (salt) | Excellent |
| Weak acids | Acceptable |
| Strong acids | Unacceptable |
| Weak alkalis | Excellent |
| Strong alkalis | Excellent |
| Organic solvents | Excellent |
| Oxidation at 500C | Limited use |
| UV radiation (sunlight) | Excellent |
| Galling resistance (adhesive wear) | Acceptable |
| Flammability | Non-flammable |
C10500 Soft Copper Corrosion resistance
| Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide | Not susceptible |
C10500 Notes
| C10500 Soft Copper Other notes |
| (s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng. |
C10500 Standards with similar compositions
| Australia: 116 to AS 1567, C11600 to AS 2738, Cu-Ag to AS 2738 |
| Europe: CW004A to CEN EN 12165, CW004A to CEN EN 12420, CW008A to CEN EN 12165, CW008A to CEN EN 12420, CW021A to CEN EN 12165 |
| International: CuAg0.1 to ISO 1634, CuAg0.1 to ISO 1638 |
| USA: C10400, C10500, C10700, C10930, C10940, C11300, C11300 to ASTM B152M, C11300 to SAE J463, C11400, C11400 to SAE J463, C11500, C11500 to SAE J463, C11600, C11600 to SAE J463, C12100, C12900, STP to ASME SB152, STP to ASTM B334, STP to ASTM B506, UNS C10400, UNS C10500, UNS C10700, UNS C10930, UNS C10940, UNS C11300, UNS C11400, UNS C11500, UNS C11600, UNS C11904, UNS C11905, UNS C11906, UNS C11907, UNS C12100, UNS C12900 |
| Tradenames: AMSIL, BOLTOMET 110, BOLTOMET 111, BOLTOMET 112, BOLTOMET 113, BOLTOMET 114, BOLTOMET 115, BOLTOMET 117, COPPER WITH SILVER, IMI 151, MITSUBISHI MKA, NORANDA 1140, NORANDA 1150, NORANDA 1160, OLIN C11300, OLIN C11400, OLIN C11600, OLIN COPPER 104 OFS, OLIN COPPER 1142 LOW OXYGEN STP, OLIN COPPER 129 FRSTP, OLIN COPPER NO. 1093, OLIN COPPER NO. 1094, OLIN COPPER, LOW OXYGEN STP 1142, OLIN COPPER, LOW OXYGEN STP 1162, PDOF NO. 104, PDOF NO. 105, PDOF NO. 107, PRYM 217, REVERE ALLOY NO. 115, REVERE NO. 113, REVERE OXYGEN FREE COPPER (2), REVERE OXYGEN FREE COPPER (3), REVERE TOUGH PITCH COPPER (1), REVERE TOUGH PITCH COPPER (2), REVERE TOUGH PITCH COPPER (3), SEYMOUR 8120, SILVER BEARING COPPER, SILVER BEARING COPPER 111, WESTERN ALLOY NO. 51, WESTERN SILVER BEARING COPPER #51 |