C10500 Silver-Bearing Oxygen-Free H.C. Copper, Hot Rolled Material Data Sheet

C10500 Silver-Bearing Oxygen-Free H.C. Copper Material Data Sheet (Wrought, Hot Rolled)

C10500 Hot Rolled Copper Overview

C10500 hot rolled copper is a wrought high conductivity copper (UNS C10500, EN CW017A), known as silver-bearing oxygen-free h.c. copper. Condition: Hot rolled. This C10500 hot rolled copper material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C10500 copper parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C10500 copper parts in-house and inspects them before shipment.

C10500 Designation

Copper Alloy: hc-Cu-OFS(hr) (UNS C10500)
ConditionHot rolled
UNS numberC10500
EN nameCW017A
ISO nameCuAg0,05(OF)

C10500 Typical uses

Magnetic windings for heavy-duty generators & motors, busbars, contacts, switches, glass to metal seals, transistor bases.

C10500 Hot Rolled Copper Composition detail

Ag (silver)0–0.02%
Cu (copper)99.9–100%

C10500 Physical properties

Density8.94–8.95g/cm3

C10500 Hot Rolled Copper Mechanical properties

Young’s modulus120–125GPa
Specific stiffness13.4–14MN.m/kg
Yield strength (elastic limit)70–90MPa
Tensile strength220–240MPa
Specific strength7.83–10.1kN.m/kg
Elongation38–42% strain
Compressive strength70–90MPa
Flexural modulus120–125GPa
Flexural strength (modulus of rupture)70–90MPa
Shear modulus44–46GPa
Bulk modulus130–135GPa
Poisson’s ratio0.34–0.35 
Shape factor30
Hardness – Vickers55–65HV
Elastic stored energy (springs)20.3–32.6kJ/m3
Fatigue strength at 10^7 cycles90–100MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
85.8–105MPa

C10500 Impact & fracture properties

Fracture toughness79.2–86.4MPa.m0.5
Toughness (G)51.2–61kJ/m2

C10500 Hot Rolled Copper Thermal properties

Melting point1080  °C
Maximum service temperature77–87°C
Minimum service temperature-273  °C
Thermal conductivity387–392W/m.°C
Specific heat capacity378–385J/kg.°C
Thermal expansion coefficient16.8–16.9µstrain/°C
Thermal shock resistance33.9–43.7°C
Thermal distortion resistance23–23.3MW/m
Latent heat of fusion200–208kJ/kg

C10500 Electrical properties

Electrical resistivity1.7–1.74µohm.cm
Electrical conductivity99.1–101%IACS
Temperature dependence of resistivity5.2–5.4/°C
Galvanic potential-0.2–-0.12V

C10500 Magnetic properties

Magnetic typeNon-magnetic

C10500 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3660–3740m/s
Mechanical loss coefficient (tan delta)4.94e-4–8.16e-4 

C10500 Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed29 m/min
Weldability
Notes: Preheating and post weld heat treatment are not required
Good

C10500 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

C10500 Hot Rolled Copper Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Not susceptible

C10500 Notes

C10500 Hot Rolled Copper Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

C10500 Standards with similar compositions

Australia: 116 to AS 1567, C11600 to AS 2738, Cu-Ag to AS 2738
Europe: CW004A to CEN EN 12165, CW004A to CEN EN 12420, CW008A to CEN EN 12165, CW008A to CEN EN 12420, CW021A to CEN EN 12165
International: CuAg0.1 to ISO 1634, CuAg0.1 to ISO 1638
USA: C10400, C10500, C10700, C10930, C10940, C11300, C11300 to ASTM B152M, C11300 to SAE J463, C11400, C11400 to SAE J463, C11500, C11500 to SAE J463, C11600, C11600 to SAE J463, C12100, C12900, STP to ASME SB152, STP to ASTM B334, STP to ASTM B506, UNS C10400, UNS C10500, UNS C10700, UNS C10930, UNS C10940, UNS C11300, UNS C11400, UNS C11500, UNS C11600, UNS C11904, UNS C11905, UNS C11906, UNS C11907, UNS C12100, UNS C12900
Tradenames: AMSIL, BOLTOMET 110, BOLTOMET 111, BOLTOMET 112, BOLTOMET 113, BOLTOMET 114, BOLTOMET 115, BOLTOMET 117, COPPER WITH SILVER, IMI 151, MITSUBISHI MKA, NORANDA 1140, NORANDA 1150, NORANDA 1160, OLIN C11300, OLIN C11400, OLIN C11600, OLIN COPPER 104 OFS, OLIN COPPER 1142 LOW OXYGEN STP, OLIN COPPER 129 FRSTP, OLIN COPPER NO. 1093, OLIN COPPER NO. 1094, OLIN COPPER, LOW OXYGEN STP 1142, OLIN COPPER, LOW OXYGEN STP 1162, PDOF NO. 104, PDOF NO. 105, PDOF NO. 107, PRYM 217, REVERE ALLOY NO. 115, REVERE NO. 113, REVERE OXYGEN FREE COPPER (2), REVERE OXYGEN FREE COPPER (3), REVERE TOUGH PITCH COPPER (1), REVERE TOUGH PITCH COPPER (2), REVERE TOUGH PITCH COPPER (3), SEYMOUR 8120, SILVER BEARING COPPER, SILVER BEARING COPPER 111, WESTERN ALLOY NO. 51, WESTERN SILVER BEARING COPPER #51