C10200 Oxygen-Free H.C. Copper, Soft Material Data Sheet
C10200 Oxygen-Free H.C. Copper Material Data Sheet (Wrought, Soft)
C10200 Soft Copper Overview
C10200 soft copper is a wrought high conductivity copper (UNS C10200, EN CW008A), known as oxygen-free h.c. copper. Condition: Soft. This C10200 soft copper material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C10200 copper parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C10200 copper parts in-house and inspects them before shipment.
Conductors, motor & generator windings, waveguides, flexible cable.
C10200 Soft Copper Composition detail
Cu (copper)
100
%
C10200 Physical properties
Density
8.94
–
8.95
g/cm3
C10200 Soft Copper Mechanical properties
Young’s modulus
120
–
125
GPa
Specific stiffness
13.4
–
14
MN.m/kg
Yield strength (elastic limit)
45
–
55
MPa
Tensile strength
210
–
230
MPa
Specific strength
5.03
–
6.15
kN.m/kg
Elongation
46
–
50
% strain
Compressive strength
45
–
55
MPa
Flexural modulus
120
–
125
GPa
Flexural strength (modulus of rupture)
45
–
55
MPa
Shear modulus
44
–
46
GPa
Bulk modulus
130
–
135
GPa
Poisson’s ratio
0.34
–
0.35
Shape factor
30
Hardness – Vickers
48
–
53
HV
Elastic stored energy (springs)
8.34
–
12.2
kJ/m3
Fatigue strength at 10^7 cycles
70
–
90
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
68.2
–
92.4
MPa
C10200 Impact & fracture properties
Fracture toughness
92.7
–
97.4
MPa.m0.5
Toughness (G)
69.9
–
77.7
kJ/m2
C10200 Soft Copper Thermal properties
Melting point
1080
°C
Maximum service temperature
77
–
87
°C
Minimum service temperature
-273
°C
Thermal conductivity
390
–
398
W/m.°C
Specific heat capacity
383
–
388
J/kg.°C
Thermal expansion coefficient
16.8
–
17.3
µstrain/°C
Thermal shock resistance
21.5
–
26.4
°C
Thermal distortion resistance
22.7
–
23.5
MW/m
Latent heat of fusion
200
–
208
kJ/kg
C10200 Electrical properties
Electrical resistivity
1.7
–
1.74
µohm.cm
Electrical conductivity
99.1
–
101
%IACS
Temperature dependence of resistivity
5.2
–
5.4
/°C
Galvanic potential
-0.2
–
-0.12
V
C10200 Magnetic properties
Magnetic type
Non-magnetic
C10200 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
3660
–
3740
m/s
Mechanical loss coefficient (tan delta)
0.00132
–
0.00198
C10200 Processing properties
Metal casting
Unsuitable
Metal cold forming
Excellent
Metal hot forming
Excellent
Metal press forming
Excellent
Metal deep drawing
Limited use
Machining speed
29 m/min
Weldability Notes: Preheating and post weld heat treatment are not required
Good
C10200 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Acceptable
Flammability
Non-flammable
C10200 Soft Copper Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Not susceptible
C10200 Notes
C10200 Soft Copper Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
C10200 Standards with similar compositions
Canada: Cu-DLP(120) to CSA
Czech Republic: Cu99.75 to CSN 423004, Cu99.85 to CSN 423003
Germany: 2.009 to DIN, Ms58 to DIN, SF-Cu to DIN
Mexico: DLP to DGN W-23
USA: BVCu-1x to AWS A5.8, C10100 to ASTM B111M, C10100 to ASTM B359M, C10100 to ASTM B640, C15150, C71630, ECu to AWS A5.6, OFXLP to ASTM B12, OFXLP to ASTM B133, UNS C14440, UNS C15150