C10100 Electrolytic Tough-Pitch H.C. Copper, Soft Material Data Sheet

C10100 Electrolytic Tough-Pitch H.C. Copper Material Data Sheet (Wrought, Soft)

C10100 Soft Copper Overview

C10100 soft copper is a wrought high conductivity copper (UNS C10100, EN CW009A), known as electrolytic tough-pitch h.c. copper. Condition: Soft. This C10100 soft copper material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C10100 copper parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C10100 copper parts in-house and inspects them before shipment.

C10100 Designation

Wrought Copper Alloy: hc-Cu-ETP(s); C101 (UNS C10100)
ConditionSoft
UNS numberC10100
EN nameCW009A
ISO nameCu-OFE
JIS (Japanese) nameC1010

C10100 Typical uses

Cables: overhead lines, motor & generator windings, busbars, contacts, stills, vats, wire, automobile radiators, architectural uses.

C10100 Soft Copper Composition detail

Cu (copper)99.9–100%
P (phosphorus)0–3e-4%
Pb (lead)0–5e-4%
S (sulfur)0–0.0015%
Sb (antimony)0–4e-4%
Zn (zinc)0–1e-4%
Other0.05  %

C10100 Physical properties

Density8.94–8.95g/cm3

C10100 Soft Copper Mechanical properties

Young’s modulus122–128GPa
Specific stiffness13.6–14.3MN.m/kg
Yield strength (elastic limit)50–70MPa
Tensile strength210–230MPa
Specific strength5.59–7.83kN.m/kg
Elongation47–50% strain
Compressive strength50–70MPa
Flexural modulus122–128GPa
Flexural strength (modulus of rupture)50–70MPa
Shear modulus44–46GPa
Bulk modulus132–138GPa
Poisson’s ratio0.34–0.35 
Shape factor30
Hardness – Vickers45–55HV
Elastic stored energy (springs)10.2–19.1kJ/m3
Fatigue strength at 10^7 cycles70–80MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
67–83.6MPa

C10100 Impact & fracture properties

Fracture toughness86.4–95MPa.m0.5
Toughness (G)59.7–72.3kJ/m2

C10100 Soft Copper Thermal properties

Melting point1080  °C
Maximum service temperature77–87°C
Minimum service temperature-273  °C
Thermal conductivity390–398W/m.°C
Specific heat capacity383–387J/kg.°C
Thermal expansion coefficient16.8–17.3µstrain/°C
Thermal shock resistance23.4–32.9°C
Thermal distortion resistance22.7–23.5MW/m
Latent heat of fusion200–208kJ/kg

C10100 Electrical properties

Electrical resistivity1.7–1.74µohm.cm
Electrical conductivity99.1–101%IACS
Temperature dependence of resistivity5.2–5.4/°C
Galvanic potential-0.2–-0.12V

C10100 Magnetic properties

Magnetic typeNon-magnetic

C10100 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3690–3780m/s
Mechanical loss coefficient (tan delta)8.16e-4–0.0016 

C10100 Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed29.3 m/min
Weldability
Notes: Preheating and post weld heat treatment are not required
Good

C10100 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

C10100 Soft Copper Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Not susceptible

C10100 Notes

C10100 Soft Copper Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

C10100 Standards with similar compositions

Australia: C10100 to AS 2738
Europe: CW021A to CEN EN 12420
Finland: Cu-DLP to SFS 2906
International: Cu-DHP to ISO 1634, Cu-DLP to ISO 1637, Cu-DLP to ISO R1337
Japan: C1011 BE/BD to JIS H3510, C1011 CB/CC to JIS H2123, C1011 P/R/T to JIS H3510, C1011 W to JIS H3510, Cathode copper to JIS H2121, Gcu to JIS Z3202
South Africa: 804 to SABS 804, 805 to SABS 805, Cu-ETP to SABS 460, Cu-FRHC to SABS 460
UK: C101 to BS 1036, C102 to BS 1037, C103 to BS 2873
USA: BVCu-1x to AWS A5.8, C10100, C10100 to AMS 4700C, C10300, C10300 to ASTM B111M, C10300 to ASTM B152M, C10300 to ASTM B187M, C10300 to ASTM B188, C10300 to ASTM B302, C10300 to ASTM B359M, C10300 to ASTM B372, C10300 to ASTM B379, C10300 to ASTM B395M, C10300 to ASTM B42, C10300 to ASTM B447, C10300 to ASTM B640, C10300 to ASTM B68M, C10300 to ASTM B743, C10300 to ASTM B75M, C10800 to ASTM B12, C10800 to ASTM B133, C10800 to ASTM B357, C11040, C12000 to ASTM B188, C12200 to ASTM B42, C14181, UNS C10100, UNS C10300, UNS C11040, UNS C14181
Tradenames: AMAX XLP, COPPER M3, COPPER, DEOXIDIZED, DLP, COPPER, DEOXIDIZED, XLP, LOW PHOSPHORUS COPPER, MUELLER 1477, OILITE COPPER, REVERE NO. 120, REVERE OXYGEN FREE EXTRA LOW PHOSPHORUS, WOLVERINE ALLOY 07