C10100 Electrolytic Tough-Pitch H.C. Copper, Hard Material Data Sheet
C10100 Electrolytic Tough-Pitch H.C. Copper Material Data Sheet (Wrought, Hard)
C10100 Hard Copper Overview
C10100 hard copper is a wrought high conductivity copper (UNS C10100, EN CW009A), known as electrolytic tough-pitch h.c. copper. Condition: Hard. This C10100 hard copper material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C10100 copper parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C10100 copper parts in-house and inspects them before shipment.
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
79.8
–
125
MPa
C10100 Impact & fracture properties
Fracture toughness
38.8
–
56.7
MPa.m0.5
Toughness (G)
11.9
–
24
kJ/m2
C10100 Hard Copper Thermal properties
Melting point
1080
°C
Maximum service temperature
77
–
87
°C
Minimum service temperature
-273
°C
Thermal conductivity
390
–
398
W/m.°C
Specific heat capacity
383
–
387
J/kg.°C
Thermal expansion coefficient
16.8
–
17.3
µstrain/°C
Thermal shock resistance
83.4
–
154
°C
Thermal distortion resistance
22.7
–
23.5
MW/m
Latent heat of fusion
200
–
208
kJ/kg
C10100 Electrical properties
Electrical resistivity
1.7
–
1.74
µohm.cm
Electrical conductivity
99.1
–
101
%IACS
Temperature dependence of resistivity
5.2
–
5.4
/°C
Galvanic potential
-0.2
–
-0.12
V
C10100 Magnetic properties
Magnetic type
Non-magnetic
C10100 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
3740
–
3890
m/s
Mechanical loss coefficient (tan delta)
3.5e-5
–
1.17e-4
C10100 Processing properties
Metal casting
Unsuitable
Metal cold forming
Excellent
Metal hot forming
Excellent
Metal press forming
Excellent
Metal deep drawing
Limited use
Machining speed
29 m/min
Weldability Notes: Preheating and post weld heat treatment are not required
Good
C10100 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Acceptable
Flammability
Non-flammable
C10100 Hard Copper Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Not susceptible
C10100 Notes
C10100 Hard Copper Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
C10100 Standards with similar compositions
Australia: C10100 to AS 2738
Europe: CW021A to CEN EN 12420
Finland: Cu-DLP to SFS 2906
International: Cu-DHP to ISO 1634, Cu-DLP to ISO 1637, Cu-DLP to ISO R1337
Japan: C1011 BE/BD to JIS H3510, C1011 CB/CC to JIS H2123, C1011 P/R/T to JIS H3510, C1011 W to JIS H3510, Cathode copper to JIS H2121, Gcu to JIS Z3202
South Africa: 804 to SABS 804, 805 to SABS 805, Cu-ETP to SABS 460, Cu-FRHC to SABS 460
UK: C101 to BS 1036, C102 to BS 1037, C103 to BS 2873
USA: BVCu-1x to AWS A5.8, C10100, C10100 to AMS 4700C, C10300, C10300 to ASTM B111M, C10300 to ASTM B152M, C10300 to ASTM B187M, C10300 to ASTM B188, C10300 to ASTM B302, C10300 to ASTM B359M, C10300 to ASTM B372, C10300 to ASTM B379, C10300 to ASTM B395M, C10300 to ASTM B42, C10300 to ASTM B447, C10300 to ASTM B640, C10300 to ASTM B68M, C10300 to ASTM B743, C10300 to ASTM B75M, C10800 to ASTM B12, C10800 to ASTM B133, C10800 to ASTM B357, C11040, C12000 to ASTM B188, C12200 to ASTM B42, C14181, UNS C10100, UNS C10300, UNS C11040, UNS C14181