Home » Gunmetal Alloys » CuSn2ZnPb (C83810) Leaded Gunmetal, Cast Material Data Sheet
CuSn2ZnPb (C83810) Leaded Gunmetal, Cast Material Data Sheet
CuSn2ZnPb (C83810) Leaded Gunmetal Material Data Sheet (Cast)
C83810 Cast Gunmetal Overview
C83810 cast gunmetal is a cast gunmetal (UNS C83810), known as leaded gunmetal. Condition: Cast. This C83810 cast gunmetal material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C83810 gunmetal castings from Turkey (Türkiye)? Modulus Metal supplies C83810 gunmetal castings with in-house CNC machining and inspects them before shipment.
C83810 Designation
CuSn2ZnPb
UNS number
C83810
ISO name
CuSn3Zn8Pb5
C83810 Typical uses
Pumps, valves, housings to resist corrosion, low-stressed bushings.
C83810 Cast Gunmetal Composition detail
Al (aluminum)
0
–
0.01
%
As (arsenic)
0
–
0.5
%
Bi (bismuth)
0
–
0.1
%
Cu (copper)
77.4
–
86.5
%
Fe (iron)
0
–
0.5
%
Ni (nickel)
0
–
2
%
Pb (lead)
4
–
6
%
Sb (antimony)
0
–
0.5
%
Si (silicon)
0
–
0.005
%
Sn (tin)
2
–
3.5
%
Zn (zinc)
7.5
–
9.5
%
C83810 Physical properties
Density
8.75
–
8.85
g/cm3
C83810 Cast Gunmetal Mechanical properties
Young’s modulus
79
–
82
GPa
Specific stiffness
8.97
–
9.33
MN.m/kg
Yield strength (elastic limit)
80
–
130
MPa
Tensile strength
180
–
270
MPa
Specific strength
9.09
–
14.8
kN.m/kg
Elongation
2
–
8
% strain
Compressive strength
80
–
130
MPa
Flexural modulus
79
–
82
GPa
Flexural strength (modulus of rupture)
80
–
130
MPa
Shear modulus
29.2
–
30.3
GPa
Bulk modulus
85.3
–
88.6
GPa
Poisson’s ratio
0.34
–
0.35
Shape factor
29
Hardness – Vickers
65
–
80
HV
Elastic stored energy (springs)
41.7
–
100
kJ/m3
Fatigue strength at 10^7 cycles
105
–
137
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
81.4
–
177
MPa
C83810 Impact & fracture properties
Fracture toughness
67.9
–
82.6
MPa.m0.5
Toughness (G)
57.7
–
84.1
kJ/m2
C83810 Cast Gunmetal Thermal properties
Melting point
927
–
1070
°C
Maximum service temperature
180
–
190
°C
Minimum service temperature
-63
–
-48
°C
Thermal conductivity
74
–
76
W/m.°C
Specific heat capacity
383
–
384
J/kg.°C
Thermal expansion coefficient
17.5
–
18.5
µstrain/°C
Thermal shock resistance
55.2
–
89.9
°C
Thermal distortion resistance
4.04
–
4.3
MW/m
Latent heat of fusion
220
–
240
kJ/kg
C83810 Electrical properties
Electrical resistivity
10.7
–
14.5
µohm.cm
Electrical conductivity
11.9
–
16.1
%IACS
Galvanic potential
-0.26
–
-0.18
V
C83810 Magnetic properties
Magnetic type
Non-magnetic
C83810 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
2990
–
3050
m/s
Mechanical loss coefficient (tan delta)
2.37e-4
–
6.25e-4
C83810 Processing properties
Metal casting
Excellent
Metal cold forming
Unsuitable
Metal hot forming
Unsuitable
Metal press forming
Unsuitable
Metal deep drawing
Unsuitable
Machining speed
122 m/min
Weldability
Unsuitable
C83810 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear) Notes: Contains lead which lubricates, improving resistance.
Excellent
Flammability
Non-flammable
C83810 Cast Gunmetal Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Susceptible
C83810 Notes
C83810 Cast Gunmetal Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
C83810 Standards with similar compositions
Australia: 838C to AS 1565, C83810A to AS 2738
Europe: CB490K to CEN EN 1982, CC490K to CEN EN 1982