CuSn10Zn2 (C90500) Admiralty Gunmetal, Cast Material Data Sheet

CuSn10Zn2 (C90500) Admiralty Gunmetal Material Data Sheet (Cast)

C90500 Cast Gunmetal Overview

C90500 cast gunmetal is a cast gunmetal (UNS C90500), known as admiralty gunmetal. Condition: Cast. This C90500 cast gunmetal material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C90500 gunmetal castings from Turkey (Türkiye)? Modulus Metal supplies C90500 gunmetal castings with in-house CNC machining and inspects them before shipment.

C90500 Designation

CuSn10Zn2
UNS numberC90500
ISO nameCuSn10Zn2
GB (Chinese) nameCuSn10Zn2
JIS (Japanese) nameBC 3

C90500 Typical uses

Pumps and valves, bearings, valve guides, marine uses.

C90500 Cast Gunmetal Composition detail

Al (aluminum)0–0.005%
Cu (copper)84.2–90%
Fe (iron)0–0.2%
Ni (nickel)0–1%
P (phosphorus)0–0.05%
Pb (lead)0–0.3%
S (sulfur)0–0.05%
Sb (antimony)0–0.2%
Si (silicon)0–0.005%
Sn (tin)9–11%
Zn (zinc)1–3%

C90500 Physical properties

Density8.75–8.85g/cm3

C90500 Cast Gunmetal Mechanical properties

Young’s modulus79–82GPa
Specific stiffness8.97–9.33MN.m/kg
Yield strength (elastic limit)130–170MPa
Tensile strength250–340MPa
Specific strength14.8–19.3kN.m/kg
Elongation5–16% strain
Compressive strength130–170MPa
Flexural modulus79–82GPa
Flexural strength (modulus of rupture)130–170MPa
Shear modulus29.2–30.3GPa
Bulk modulus85.3–88.6GPa
Poisson’s ratio0.34–0.35 
Shape factor28
Hardness – Vickers70–95HV
Elastic stored energy (springs)107–177kJ/m3
Fatigue strength at 10^7 cycles130–159MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
106–195MPa

C90500 Impact & fracture properties

Fracture toughness59.4–67.9MPa.m0.5
Toughness (G)44–57.1kJ/m2

C90500 Cast Gunmetal Thermal properties

Melting point887–1040°C
Maximum service temperature200–210°C
Minimum service temperature-63–-48°C
Thermal conductivity62–64W/m.°C
Specific heat capacity383–384J/kg.°C
Thermal expansion coefficient17.5–18.5µstrain/°C
Thermal shock resistance89.5–118°C
Thermal distortion resistance3.39–3.61MW/m
Latent heat of fusion220–240kJ/kg

C90500 Electrical properties

Electrical resistivity15.8–17.4µohm.cm
Electrical conductivity9.91–10.9%IACS
Galvanic potential-0.24–-0.16V

C90500 Magnetic properties

Magnetic typeNon-magnetic

C90500 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity2990–3050m/s
Mechanical loss coefficient (tan delta)1.38e-4–2.37e-4 

C90500 Processing properties

Metal castingAcceptable
Metal cold formingUnsuitable
Metal hot formingUnsuitable
Metal press formingUnsuitable
Metal deep drawingUnsuitable
Machining speed39.6 m/min
WeldabilityUnsuitable

C90500 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Excellent
FlammabilityNon-flammable

C90500 Cast Gunmetal Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Slightly susceptible

C90500 Notes

C90500 Cast Gunmetal Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

C90500 Standards with similar compositions

Czech Republic: CuSn10Zn2 to CSN 423138
Germany: 2.1086 to DIN, 2.1087 to DIN 17656, GB-CuSn10Zn to DIN 17656, G-CuSn10Zn to DIN
Japan: CAC403 to JIS H5120, CAC403C to JIS H5121
Norway: 16512 to NS 16512
USA: C90500, C90500 to AMS 4845, C90500 to ASTM B22, C90500 to ASTM B271, C90500 to ASTM B30, C90500 to ASTM B584, C90500 to ASTM B763, C90500 to QQ C-390, C90500 to SAE J462, UNS C90500
Venezuela: C90500 to COPANT 801
Tradenames: FEDERALOY F-1, LILY BRAND NO. 1