Home » Gunmetal Alloys » CuPb5Sn5Zn5 (85-5-5-5) (C83600) Leaded Gunmetal, Cast Material Data Sheet
CuPb5Sn5Zn5 (85-5-5-5) (C83600) Leaded Gunmetal, Cast Material Data Sheet
CuPb5Sn5Zn5 (85-5-5-5) (C83600) Leaded Gunmetal Material Data Sheet (Cast)
C83600 Cast Gunmetal Overview
C83600 cast gunmetal is a cast gunmetal (UNS C83600, EN CC491K), known as leaded gunmetal. Condition: Cast. This C83600 cast gunmetal material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C83600 gunmetal castings from Turkey (Türkiye)? Modulus Metal supplies C83600 gunmetal castings with in-house CNC machining and inspects them before shipment.
C83600 Designation
CuPb5Sn5Zn5 (85-5-5-5)
UNS number
C83600
EN name
CC491K
ISO name
CuPb5Sn5Zn5
JIS (Japanese) name
BC 6 / BC ln 6
C83600 Typical uses
Pumps, valves, housings to resist corrosion, low-stressed bushings.
C83600 Cast Gunmetal Composition detail
Al (aluminum)
0
–
0.005
%
Cu (copper)
80.3
–
88
%
Fe (iron)
0
–
0.3
%
Ni (nickel)
0
–
1
%
P (phosphorus)
0
–
0.05
%
Pb (lead)
4
–
6
%
S (sulfur)
0
–
0.08
%
Sb (antimony)
0
–
0.25
%
Si (silicon)
0
–
0.005
%
Sn (tin)
4
–
6
%
Zn (zinc)
4
–
6
%
C83600 Physical properties
Density
8.75
–
8.85
g/cm3
C83600 Cast Gunmetal Mechanical properties
Young’s modulus
79
–
82
GPa
Specific stiffness
8.97
–
9.33
MN.m/kg
Yield strength (elastic limit)
110
–
140
MPa
Tensile strength
200
–
280
MPa
Specific strength
12.5
–
15.9
kN.m/kg
Elongation
6
–
15
% strain
Compressive strength
110
–
140
MPa
Flexural modulus
79
–
82
GPa
Flexural strength (modulus of rupture)
110
–
140
MPa
Shear modulus
29.2
–
30.3
GPa
Bulk modulus
85.3
–
88.6
GPa
Poisson’s ratio
0.34
–
0.35
Shape factor
29
Hardness – Vickers
80
–
95
HV
Elastic stored energy (springs)
76.1
–
120
kJ/m3
Fatigue strength at 10^7 cycles
113
–
140
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
90.6
–
175
MPa
C83600 Impact & fracture properties
Fracture toughness
65.5
–
73.1
MPa.m0.5
Toughness (G)
53.4
–
66.3
kJ/m2
C83600 Cast Gunmetal Thermal properties
Melting point
927
–
1050
°C
Maximum service temperature
180
–
190
°C
Minimum service temperature
-63
–
-48
°C
Thermal conductivity
70
–
75
W/m.°C
Specific heat capacity
383
–
384
J/kg.°C
Thermal expansion coefficient
17.5
–
18.5
µstrain/°C
Thermal shock resistance
75.7
–
97
°C
Thermal distortion resistance
3.85
–
4.21
MW/m
Latent heat of fusion
220
–
240
kJ/kg
C83600 Electrical properties
Electrical resistivity
11.5
–
17.4
µohm.cm
Electrical conductivity
9.91
–
15
%IACS
Galvanic potential
-0.25
–
-0.17
V
C83600 Magnetic properties
Magnetic type
Non-magnetic
C83600 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
2990
–
3050
m/s
Mechanical loss coefficient (tan delta)
2.04e-4
–
3.31e-4
C83600 Processing properties
Metal casting
Excellent
Metal cold forming
Unsuitable
Metal hot forming
Unsuitable
Metal press forming
Unsuitable
Metal deep drawing
Unsuitable
Machining speed
79.2 m/min
Weldability
Unsuitable
C83600 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear) Notes: Contains lead which lubricates, improving resistance.
Excellent
Flammability
Non-flammable
C83600 Cast Gunmetal Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Susceptible
C83600 Notes
C83600 Cast Gunmetal Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
C83600 Standards with similar compositions
Australia: C83600A to AS 2738
Czech Republic: CuSn5PbZn5 to CSN 423135
Europe: CB491K to CEN EN 1982, CC491K to CEN EN 1982
Germany: 2.1096 to DIN, G-CuSn5ZnPb to DIN
International: CuPb5Sn5Zn5 to ISO 4382-1
Japan: CAC406 to JIS H5120, CAC406C to JIS H5121
Norway: 16530 to NS 16530
USA: C83600, C83600 to ASTM B271, C83600 to ASTM B30, C83600 to ASTM B584, C83600 to ASTM B62, UNS C83600