17-7PH TH1050 Stainless Steel Material Data Sheet

17-7PH TH1050 Stainless Steel Material Data Sheet (Semi-austenitic, Precipitation Hardened)

17-7PH TH1050 Stainless Steel Overview

17-7PH TH1050 stainless steel is a semi-austenitic precipitation hardening stainless steel (UNS S17700) in the wrought form. Condition: TH1050 (Solution annealed; precipitation (age) hardened at 566°C; air cooled). This 17-7PH TH1050 stainless steel material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for 17-7PH parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined 17-7PH parts in-house and inspects them before shipment.

17-7PH Designation

17-7PH, wrought
ConditionTH1050 (Solution annealed; precipitation (age) hardened at 566°C; air cooled)
UNS numberS17700
US name~ASTM S17700, ~ASME 631, ~AMS 5529, ~AMS 5528
EN name~X7CrNiAl17-7
EN number~1.4568
ISO name~X7CrNiAl17-7, ~X7CrNial17-7
JIS (Japanese) nameSUS631

17-7PH Typical uses

Processing of potentially corrosive liquids e.g. chemicals/oil/beverages/sewage, structural uses in corrosive environments, e.g. nuclear plants, ships, offshore oil installations, underwater cables and pipes

17-7PH TH1050 Stainless Steel Composition detail

Al (aluminum)0.75–1.5%
C (carbon)0–0.09%
Cr (chromium)16–18%
Fe (iron)70.6–76.8%
Mn (manganese)0–1%
Ni (nickel)6.5–7.75%
P (phosphorus)0–0.04%
S (sulfur)0–0.03%
Si (silicon)0–1%

17-7PH Physical properties

Density7.6–7.68g/cm3

17-7PH TH1050 Stainless Steel Mechanical properties

Young’s modulus200–210GPa
Specific stiffness26.2–27.5MN.m/kg
Yield strength (elastic limit)1030–1150MPa
Tensile strength1220–1370MPa
Specific strength135–151kN.m/kg
Elongation4–6% strain
Compressive strength1100–1280MPa
Flexural modulus200–210GPa
Flexural strength (modulus of rupture)1030–1150MPa
Shear modulus79–83.1GPa
Bulk modulus152–159GPa
Poisson’s ratio0.28–0.291 
Shape factor22
Hardness – Vickers350–500HV
Hardness – Rockwell B100–120HRB
Hardness – Rockwell C40–45HRC
Hardness – Brinell375–415HB
Elastic stored energy (springs)2610–3230kJ/m3
Fatigue strength at 10^7 cycles477–569MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
454–598MPa

17-7PH Impact & fracture properties

Fracture toughness38.7–47.3MPa.m0.5
Toughness (G)7.36–10.8kJ/m2

17-7PH TH1050 Stainless Steel Thermal properties

Melting point1400–1440°C
Maximum service temperature282–316°C
Minimum service temperature-73–-43°C
Thermal conductivity16.4–17.8W/m.°C
Specific heat capacity480–530J/kg.°C
Thermal expansion coefficient11.7–12.3µstrain/°C
Thermal shock resistance416–473°C
Thermal distortion resistance1.36–1.49MW/m
Latent heat of fusion260–285kJ/kg

17-7PH Electrical properties

Electrical resistivity78–88µohm.cm
Electrical conductivity1.96–2.21%IACS
Galvanic potential-0.19–-0.11V

17-7PH Magnetic properties

Magnetic typeMagnetic

17-7PH Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5110–5250m/s
Mechanical loss coefficient (tan delta)3.1e-4–6.6e-4 

17-7PH Processing properties

Metal castingUnsuitable
Metal cold formingAcceptable
Metal hot formingAcceptable
Metal press formingAcceptable
Metal deep drawingUnsuitable
Machining speed10.4 m/min
Weldability
Notes: Preheating is not required, post weld heat treatment is required
Good
Weldability – MIGGood
Weldability – plasmaGood
Weldability – SAWNot recommended
Weldability – TIGGood
BrazeabilityGood
Carbon equivalency0.642 – 0.886

17-7PH Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsExcellent
Strong acidsAcceptable
Weak alkalisExcellent
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CExcellent
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Aluminum bronze is the most suitable mating material to minimize galling.
Limited use
FlammabilityNon-flammable

17-7PH TH1050 Stainless Steel Corrosion resistance

Pitting resistance equivalent number (PREN)16 – 18
Pitting and crevice corrosionLow (<20)
Stress corrosion cracking
Note: Rated in chloride; Other susceptible environments: Hydrogen sulfide
Susceptible
Intergranular (weld line) corrosionGood
Inorganic acidsRestricted
Organic acidsModerate
AlkalisModerate
Humidity / waterExcellent
Sea waterRestricted
Sour oil and gasRestricted

17-7PH Standards with similar compositions

China: 0Cr17Ni7Al to GB 1220, 0Cr17Ni7Al to GB 1221, 0Cr17Ni7Al to GB 4237, 0Cr17Ni7Al to GB 4238, 0Cr17Ni7Al to GB/T 3280, 0Cr17Ni7Al to GB/T 4231, 0Cr17Ni7Al to GB/T 4239, 0Cr17Ni7Al to GB/T 4356, 0Cr17Ni7Al to GB/T 6725
France: Z8CNA17.07 to AFNOR NF A35-581
Germany: 1.4568 to DIN EN 10088
International: X7CrNiAl17-7 to ISO 16143-1, X7CrNial17-7 to ISO 16143-2, X7CrNiAl17-7 to ISO 16143-3, X7CrNiAl17-7 to ISO 6931-1, X7CrNiAl17-7 to ISO 6931-2
Japan: SUS631 to JIS G4303, SUS631 to JIS G4304, SUS631 to JIS G4305, SUS631 to JIS G4306, SUS631 to JIS G4307, SUS631-CSP to JIS G4313, SUS631J1 to JIS G4308
South Korea: STS 631 to KS D 3706, STS 631-CSP to KS D 3534, STS 631J1 to KS D 3535, STS631 to KS D 3698, STS631 to KS D 3705, STS631J1 to KS D 3702
Sweden: 2388 to SS 142388
UK: 301S81 to BS 2056, X7CrNiAl17-7 to BS EN 10088-1, X7CrNiAl17-7 to BS EN 10088-2, X7CrNiAl17-7 to BS EN 10088-3, X7CrNiAl17-7 to BS EN 10270-3
USA: 17-7 PH to MIL-S-25043, 17-7PH to SAE J467, 5528 to AMS 5528, 5529 to AMS 5529, 5568 to AMS 5568, 5644 to AMS 5644, 5673 to AMS 5673, 5678 to AMS 5678, 62 to ASTM A579, S17700 to ASTM A313/A313M, S17700 to ASTM A564/A564M, S17700 to ASTM A693, S17700 to ASTM A705/A705M-95, S17700 to ASTM A959, UNS S17700, UNS S17780
Tradenames: AL 17-7, KRUPP WL 1.4564, MCKAY 17-7 PH, NIROSTA 4568