AISI 1022 Annealed Material Data Sheet
AISI 1022 Annealed Overview
| AISI 1022 annealed is AISI 1022 low carbon steel (UNS G10220, EN 2C22) in the annealed condition. This AISI 1022 annealed material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 1022 conditions in our AISI 1022 yield, tensile and hardness comparison. Looking for AISI 1022 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1022 steel parts in-house and inspects them before shipment. |
AISI 1022 Annealed Designation
| AISI 1022 | |
| Condition | Annealed |
| UNS number | G10220 |
| US name | ASTM MTX1020, ASTM 1022, ASME G10220, ASME G10210, ~SAE 050W, ~SAE 045Z, ~SAE 045Y, ~SAE 045X, ~SAE 045W, ~SAE 040S, ~SAE 040C, ~SAE 040B, ~SAE 040A |
| EN name | 2C22, 055M15, ~S270GP |
| EN number | ~1.0023 |
| ISO name | ~R44, ~HR275 Class B, ~E275 Quality A |
| GB (Chinese) name | ~ML22Mn |
| JIS (Japanese) name | ~SWRCH22A, ~STK500, ~SNR400A, ~SN 400 A, ~SM400A, ~SHK 400 M, ~SG 295 |
AISI 1022 Annealed Typical uses
| General construction, general mechanical engineering, automotive, tools, axles, gears, springs. |
AISI 1022 Annealed Composition detail
| C (carbon) | 0.18 | – | 0.23 | % |
| Fe (iron) | 98.7 | – | 99.1 | % |
| Mn (manganese) | 0.7 | – | 1 | % |
| P (phosphorus) | 0 | – | 0.04 | % |
| S (sulfur) | 0 | – | 0.05 | % |
AISI 1022 Annealed Physical properties
| Density | 7.8 | – | 7.9 | g/cm3 |
AISI 1022 Annealed Mechanical properties
| Young’s modulus | 205 | – | 215 | GPa |
| Specific stiffness | 26.1 | – | 27.4 | MN.m/kg |
| Yield strength (elastic limit) | 285 | – | 350 | MPa |
| Tensile strength | 380 | – | 475 | MPa |
| Specific strength | 36.3 | – | 44.6 | kN.m/kg |
| Elongation | 28 | – | 42 | % strain |
| Compressive strength | 285 | – | 350 | MPa |
| Flexural modulus | 205 | – | 215 | GPa |
| Flexural strength (modulus of rupture) | 285 | – | 350 | MPa |
| Shear modulus | 79 | – | 84 | GPa |
| Bulk modulus | 158 | – | 175 | GPa |
| Poisson’s ratio | 0.285 | – | 0.295 | |
| Shape factor | 60 | |||
| Hardness – Vickers | 130 | – | 160 | HV |
| Elastic stored energy (springs) | 195 | – | 289 | kJ/m3 |
| Fatigue strength at 10^7 cycles | 217 | – | 255 | MPa |
| Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles | 186 | – | 297 | MPa |
AISI 1022 Annealed Impact & fracture properties
| Fracture toughness | 42 | – | 67 | MPa.m0.5 |
| Toughness (G) | 8.78 | – | 20.5 | kJ/m2 |
AISI 1022 Annealed Thermal properties
| Melting point | 1480 | – | 1520 | °C |
| Maximum service temperature | 340 | – | 356 | °C |
| Minimum service temperature | -68 | – | -43 | °C |
| Thermal conductivity | 50 | – | 54 | W/m.°C |
| Specific heat capacity | 465 | – | 505 | J/kg.°C |
| Thermal expansion coefficient | 12 | – | 13 | µstrain/°C |
| Thermal shock resistance | 108 | – | 135 | °C |
| Thermal distortion resistance | 3.94 | – | 4.4 | MW/m |
| Latent heat of fusion | 270 | – | 275 | kJ/kg |
AISI 1022 Annealed Electrical properties
| Electrical resistivity | 16 | – | 18 | µohm.cm |
| Electrical conductivity | 9.58 | – | 10.8 | %IACS |
| Galvanic potential | -0.52 | – | -0.44 | V |
AISI 1022 Annealed Magnetic properties
| Magnetic type | Magnetic |
AISI 1022 Annealed Optical, aesthetic and acoustic properties
| Transparency | Opaque | |||
| Acoustic velocity | 5110 | – | 5240 | m/s |
| Mechanical loss coefficient (tan delta) | 0.00103 | – | 0.00128 | |
AISI 1022 Annealed Processing properties
| Metal casting | Unsuitable |
| Metal cold forming | Acceptable |
| Metal hot forming | Excellent |
| Metal press forming | Acceptable |
| Metal deep drawing | Limited use |
| Machining speed | 39.6 m/min |
| Weldability Notes: Preheating and post weld heat treatments are required | Good |
| Carbon equivalency | 0.297 – 0.397 |
AISI 1022 Annealed Durability
| Water (fresh) | Acceptable |
| Water (salt) | Limited use |
| Weak acids | Limited use |
| Strong acids | Unacceptable |
| Weak alkalis | Acceptable |
| Strong alkalis | Limited use |
| Organic solvents | Excellent |
| Oxidation at 500C | Acceptable |
| UV radiation (sunlight) | Excellent |
| Galling resistance (adhesive wear) Notes: Aluminum bronze is the most suitable mating material to minimize galling. | Limited use |
| Flammability | Non-flammable |
AISI 1022 Annealed Corrosion resistance
| Stress corrosion cracking Note: Rated in chloride; Other susceptible environments: Nitrate, hydroxide, carbonate, ammonia | Not susceptible |
AISI 1022 Annealed Standards with similar compositions
| Argentina: IRAM 1018 to IAS |
| Canada: A to CSA B193, B193 to CSA B193 |
| China: ML22Mn to GB/T 6478 |
| India: 20C8 to IS 11169/1, 20C8 to IS 1570/2/1, C20 to IS 1570/2/1, Fe 380 to IS 12367, Grade 7M to IS 7887, Grade 7M to IS 8952, Grade 8M to IS 7887, Grade 8M to IS 8952 |
| Japan: SWRCH22A to JIS G3507 |
| Mexico: 1018 to NMX-B-301, 1019 to NMX-B-301, 1021 to NMX-B-301, 1022 to NMX-B-301, MTX1020 to NMX-B-201, MTX1020 to NMX-B-203-SCFI |
| Pan America: 1018 to COPANT 331, 1018 to COPANT 333, 1019 to COPANT 333, 1021 to COPANT 331, 1021 to COPANT 333, 1022 to COPANT 330, 1022 to COPANT 331, 1022 to COPANT 333 |
| South Korea: SWRCH22A to KS D 3592 |
| UK: 170H20 to BS 970/1 |
| USA: 1018, 1018 Class A to ASTM A311/A311M, 1018 to ASTM A29/A29M, 1018 to ASTM A519, 1018 to ASTM A787, 1018 to FED QQ-S-698, 1018 to FED QQ-W-461H, 1018 to MIL-R-8814, 1018 to SAE J403, 1019, 1019 Mod, 1019 to ASTM A29/A29M, 1019 to ASTM A512-96, 1019 to ASTM A513, 1019 to ASTM A519, 1019 to ASTM A568/A568M, 1019 to ASTM A787, 1019 to FED QQ-S-633A, 1019 to SAE J1249, 1019 to SAE J403, 1021, 1021 to ASTM A29/A29M, 1021 to ASTM A512-96, 1021 to ASTM A513, 1021 to ASTM A519, 1021 to ASTM A568/A568M, 1021 to ASTM A787, 1021 to SAE J403, 1022, 1022 Mod, 1022 to ASTM A29/A29M, 1022 to ASTM A513, 1022 to ASTM A519, 1022 to ASTM A568/A568M, 1022 to DoD-F-24669/1, 1022 to SAE J403, 10L18, G10180 to ASTM A510/A510M, G10180 to ASTM A576-90b, G10180 to ASTM A830/A830M, G10190 to ASTM A510/A510M, G10190 to ASTM A576-90b, G10190 to ASTM A830/A830M, G10210 to ASTM A510/A510M, G10210 to ASTM A576-90b, G10210 to ASTM A830/A830M, G10220 to ASTM A510/A510M, G10220 to ASTM A576-90b, G10220 to ASTM A830/A830M, Grade B to ASTM A595, HT to MIL-S-16113, MIL-R-908 to MIL-R-908, MIL-S-20166 to MIL-S-20166B, MIL-S-7809 to MIL-S-7809, MTX1020 to ASTM A512-96, MTX1020 to ASTM A513, MTX1020 to ASTM A519, MTX1020 to ASTM A787, UNS G10180, UNS G10180 to UNS, UNS G10190, UNS G10190 to UNS, UNS G10210, UNS G10210 to UNS, UNS G10220, UNS G10220 to UNS, UNS K02005 |
| Tradenames: AMERHEAD C-1018, GREDE 31, HI-YIELD 42, JESSOP A-3, LASALLE 1018, LASALLE 1020-90, MANGANESE SCREW STOCK, MARINER, MARREL 50SS, NO. 1020-90 STEEL, SANDVIK 4L7, SWB-22M3, TISCON, UGINE B21, USS 2090, USS B24 |