Bronze CuAl10Fe5Ni5 Mechanical Properties (C95820, cast aluminum bronze)

Designation
CuAl10Fe5Ni5
UNS numberC95820
EN nameCC333G
ISO nameCuAl10Fe5Ni4
GB (Chinese) nameCuAl9Fe4Ni4Mn2
JIS (Japanese) nameAl BC 3

Bronze CuAl10Fe5Ni5 Mechanical Properties (C95820, cast aluminum bronze)

Young’s modulus110–113GPa
Specific stiffness14.2–15.2MN.m/kg
Yield strength (elastic limit)250–300MPa
Tensile strength640–700MPa
Specific strength32.8–39.7kN.m/kg
Elongation13–20% strain
Compressive strength250–300MPa
Flexural modulus110–113GPa
Flexural strength (modulus of rupture)250–300MPa
Shear modulus40.7–41.8GPa
Bulk modulus119–122GPa
Poisson’s ratio0.34–0.35 
Shape factor25   
Hardness – Vickers140–180HV
Elastic stored energy (springs)282–401kJ/m^3
Fatigue strength at 10^7 cycles240–254MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles223–273MPa

MODULUS METAL
Sand Casting in Turkey, Permanent Mold Casting in Turkey, Gravity Die Casting in Turkey, Pressure Die Casting in Turkey, High-Pressure Die Casting in Turkey, Investment Casting in Turkey, Foundry in Turkey, Plastic Injection Molding in Turkey, Press Bending ( Press Brake) Products in Turkey, Laser and Plasma Cutting in Turkey, Welded Construction in Turkey, Heat Treated, CNC Machined Products Manufacturer in Turkey