17-4PH vs 15-5PH Stainless Steel: Strength, Hardness, Toughness and Corrosion Compared (H900 to H1150M)

17-4PH or 15-5PH? This 17-4PH vs 15-5PH comparison puts the two grades side by side using only the values in our 17-4PH and 15-5PH material data sheets: chemical composition, yield strength, tensile strength, hardness, elongation, fracture toughness, fatigue strength and machining speed, condition by condition. Differences are calculated from the mid-point of each range and show 15-5PH relative to 17-4PH.

Both grades are compared in the same seven aging conditions, from H900 (aged at 482°C, highest strength) to H1150M (double aged, softest). Hardness is compared in Rockwell C, because the Vickers hardness in these data sheets is given as one wide range for all conditions. Data note: the 17-4PH H1150M data sheet lists a fracture toughness of 29.7–36.3 MPa·m0.5, far below the 17-4PH H1150 value and the 15-5PH H1150M value. It is shown as given in the data sheet, but it is left out of the average differences below.

17-4PH vs 15-5PH Chemical Composition

Element (%)17-4PH15-5PH
C0–0.070–0.07
Cr15–17.514–15.5
Ni3–53.5–5.5
Cu3–52.5–4.5
Nb0.15–0.40.15–0.4
Mn0–10–1
Si0–10–1
P0–0.040–0.04
S0–0.030–0.03

17-4PH vs 15-5PH Yield strength

Condition17-4PH (MPa)15-5PH (MPa)15-5PH vs 17-4PH
H9001170–13001170–1300+0%
H9251070–11801070–1180+0%
H10251000–1110986–1090-2%
H1075862–986862–953-2%
H1100793–876793–876+0%
H1150690–793724–800+3%
H1150M517–572517–571-0%

17-4PH   15-5PH. Dark bar = minimum, light bar = maximum of the range.

17-4PH vs 15-5PH Yield strength (MPa)17-4PH H9001170–130015-5PH H9001170–130017-4PH H9251070–118015-5PH H9251070–118017-4PH H10251000–111015-5PH H1025986–109017-4PH H1075862–98615-5PH H1075862–95317-4PH H1100793–87615-5PH H1100793–87617-4PH H1150690–79315-5PH H1150724–80017-4PH H1150M517–57215-5PH H1150M517–571

17-4PH vs 15-5PH Tensile strength

Condition17-4PH (MPa)15-5PH (MPa)15-5PH vs 17-4PH
H9001310–14501310–1450+0%
H9251170–13001170–1300+0%
H10251070–11801060–1170-1%
H1075986–11001000–1110+1%
H1100965–1070965–1070+0%
H1150862–1020931–1030+4%
H1150M793–876793–876+0%
17-4PH vs 15-5PH Tensile strength (MPa)17-4PH H9001310–145015-5PH H9001310–145017-4PH H9251170–130015-5PH H9251170–130017-4PH H10251070–118015-5PH H10251060–117017-4PH H1075986–110015-5PH H10751000–111017-4PH H1100965–107015-5PH H1100965–107017-4PH H1150862–102015-5PH H1150931–103017-4PH H1150M793–87615-5PH H1150M793–876

17-4PH vs 15-5PH Hardness

Condition17-4PH (HRC)15-5PH (HRC)15-5PH vs 17-4PH
H90041–4742–47+1%
H92540–4539–44-2%
H102536–4138–42+4%
H107531–3731–38+1%
H110033–3732–37-1%
H115028–3528–36+2%
H1150M29–3327–31-6%
17-4PH vs 15-5PH Hardness (HRC)17-4PH H90041–4715-5PH H90042–4717-4PH H92540–4515-5PH H92539–4417-4PH H102536–4115-5PH H102538–4217-4PH H107531–3715-5PH H107531–3817-4PH H110033–3715-5PH H110032–3717-4PH H115028–3515-5PH H115028–3617-4PH H1150M29–3315-5PH H1150M27–31

17-4PH vs 15-5PH Elongation

Condition17-4PH (%)15-5PH (%)15-5PH vs 17-4PH
H90013.9–16.113–15.1-6%
H92514.3–16.713–15.1-9%
H102514.8–17.213.9–16.1-6%
H107515.7–18.314.8–17.2-6%
H110017.1–19.915.7–18.3-8%
H115018.5–21.517.6–20.4-5%
H1150M20.4–23.720.4–23.7+0%

17-4PH vs 15-5PH Fracture toughness

Condition17-4PH (MPa·m0.5)15-5PH (MPa·m0.5)15-5PH vs 17-4PH
H90047.3–57.879.7–97.4+69%
H92578.3–95.783.7–102+7%
H1025116–14299.1–121-15%
H1075130–158107–130-18%
H1100138–168121–147-12%
H1150161–197134–164-17%
H1150M29.7–36.3273–333+818%
17-4PH vs 15-5PH Fracture toughness (MPa√m)17-4PH H90047.3–57.815-5PH H90079.7–97.417-4PH H92578.3–95.715-5PH H92583.7–10217-4PH H1025116–14215-5PH H102599.1–12117-4PH H1075130–15815-5PH H1075107–13017-4PH H1100138–16815-5PH H1100121–14717-4PH H1150161–19715-5PH H1150134–16417-4PH H1150M29.7–36.315-5PH H1150M273–333

17-4PH vs 15-5PH Fatigue strength at 107 cycles

Condition17-4PH (MPa)15-5PH (MPa)15-5PH vs 17-4PH
H900364–542364–542+0%
H925364–542364–542+0%
H1025364–542364–542+0%
H1075364–542364–542+0%
H1100364–542364–542+0%
H1150364–542364–542+0%
H1150M364–542364–542+0%

17-4PH vs 15-5PH Machining speed

Condition17-4PH (m/min)15-5PH (m/min)15-5PH vs 17-4PH
H90012.212.2+0%
H92512.812.8+0%
H102513.413.1-2%
H107513.713.4-2%
H110013.713.7+0%
H115014.314-2%
H1150M14.914.9+0%

17-4PH vs 15-5PH Weldability, Processing and Corrosion

Property17-4PH15-5PH
Pitting resistance equivalent number (PREN)15–17.514–15.5
Stress corrosion cracking (H900)Slightly susceptibleSlightly susceptible
Stress corrosion cracking (H1150)SusceptibleNot susceptible
Sea waterRestrictedRestricted
WeldabilityGoodGood
Metal cold formingLimited useLimited use
Carbon equivalency0.65–0.970.608–0.895

17-4PH vs 15-5PH: Key Differences

Tensile strength is practically the same for 17-4PH and 15-5PH (average difference +1% across 7 matched conditions). Yield strength is practically the same for 17-4PH and 15-5PH (average difference +0% across 7 matched conditions). Fracture toughness depends on the condition: 15-5PH is 69% tougher than 17-4PH in H900, but 18% less tough in H1075. Machining speed is practically the same for 17-4PH and 15-5PH (average difference -1% across 7 matched conditions). On average across 7 matched conditions, 15-5PH has 6% lower elongation than 17-4PH.

17-4PH vs 15-5PH FAQ

Is 15-5PH stronger than 17-4PH?

No, in our data sheets the strength is practically the same in every matched condition. At H900 both have a yield strength of 1170–1300 MPa and tensile strength of 1310–1450 MPa.

Is 15-5PH tougher than 17-4PH?

At H900, yes: 15-5PH has a fracture toughness of 79.7–97.4 MPa·m^0.5 vs 47.3–57.8 for 17-4PH. In the H1025 to H1150 conditions, however, 17-4PH shows the higher values in our data sheets.

What is the difference between 17-4PH and 15-5PH composition?

17-4PH contains 15–17.5% chromium and 3–5% nickel; 15-5PH contains 14–15.5% chromium and 3.5–5.5% nickel. Copper is 3–5% vs 2.5–4.5%.

Which has better corrosion resistance, 17-4PH or 15-5PH?

Our data sheets give a PREN of 15–17.5 for 17-4PH and 14–15.5 for 15-5PH, and the same ratings for sea water (Restricted) and humidity/water.

What is the hardness of 17-4PH H900 and H1150?

In our data sheets 17-4PH H900 is 41–47 HRC and 17-4PH H1150 is 28–35 HRC.

17-4PH and 15-5PH Material Data Sheets

17-4PH H900 | 17-4PH H925 | 17-4PH H1025 | 17-4PH H1075 | 17-4PH H1100 | 17-4PH H1150 | 17-4PH H1150M | All 17-4PH conditions

15-5PH H900 | 15-5PH H925 | 15-5PH H1025 | 15-5PH H1075 | 15-5PH H1100 | 15-5PH H1150 | 15-5PH H1150M | All 15-5PH conditions

Need 17-4PH or 15-5PH parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined precipitation hardening stainless steel parts in-house, aged to the condition you specify, and inspects them before shipment.