AISI 4130 vs 4140 Steel: Composition, Strength, Hardness and Machinability Compared

AISI 4130 or AISI 4140? This AISI 4130 vs AISI 4140 comparison puts the two grades side by side using only the values in our AISI 4130 and AISI 4140 material data sheets: chemical composition, yield strength, tensile strength, hardness, elongation, fracture toughness, fatigue strength and machining speed, condition by condition. Differences are calculated from the mid-point of each range and show AISI 4140 relative to AISI 4130.

Note on the heat treatment data: in these data sheets the AISI 4130 quenched and tempered values are for water quenching, while the AISI 4140 values are for oil quenching, and the AISI 4130 normalized data sheet is for air melted material. The rows are matched by tempering temperature, so read the quenched and tempered differences with the quench medium in mind.

AISI 4130 vs AISI 4140 Chemical Composition

Element (%)AISI 4130AISI 4140
C0.28–0.330.38–0.43
Mn0.4–0.60.75–1
Si0.15–0.350.15–0.35
Cr0.8–1.10.8–1.1
Mo0.15–0.250.15–0.25
Ni——
P0–0.0350–0.035
S0–0.040–0.04

AISI 4130 vs AISI 4140 Yield strength

ConditionAISI 4130 (MPa)AISI 4140 (MPa)AISI 4140 vs AISI 4130
Annealed320–400370–460+15%
Normalized483–534595–715+29%
Q&T 205°C1320–16101480–1810+12%
Q&T 315°C1240–15201290–1580+4%
Q&T 425°C1070–13201020–1260-5%
Q&T 540°C820–1000750–920-8%
Q&T 650°C630–775595–715-7%

AISI 4130   AISI 4140. Dark bar = minimum, light bar = maximum of the range.

AISI 4130 vs AISI 4140 Yield strength (MPa)4130 Annealed320–4004140 Annealed370–4604130 Normalized483–5344140 Normalized595–7154130 Q&T 205°C1320–16104140 Q&T 205°C1480–18104130 Q&T 315°C1240–15204140 Q&T 315°C1290–15804130 Q&T 425°C1070–13204140 Q&T 425°C1020–12604130 Q&T 540°C820–10004140 Q&T 540°C750–9204130 Q&T 650°C630–7754140 Q&T 650°C595–715

AISI 4130 vs AISI 4140 Tensile strength

ConditionAISI 4130 (MPa)AISI 4140 (MPa)AISI 4140 vs AISI 4130
Annealed500–620595–720+17%
Normalized621–686915–1130+56%
Q&T 205°C1450–17701600–1950+10%
Q&T 315°C1350–16501400–1710+4%
Q&T 425°C1150–14101120–1380-2%
Q&T 540°C925–1140855–1050-8%
Q&T 650°C730–895680–840-6%
AISI 4130 vs AISI 4140 Tensile strength (MPa)4130 Annealed500–6204140 Annealed595–7204130 Normalized621–6864140 Normalized915–11304130 Q&T 205°C1450–17704140 Q&T 205°C1600–19504130 Q&T 315°C1350–16504140 Q&T 315°C1400–17104130 Q&T 425°C1150–14104140 Q&T 425°C1120–13804130 Q&T 540°C925–11404140 Q&T 540°C855–10504130 Q&T 650°C730–8954140 Q&T 650°C680–840

AISI 4130 vs AISI 4140 Hardness

ConditionAISI 4130 (HV)AISI 4140 (HV)AISI 4140 vs AISI 4130
Annealed145–185183–223+23%
Normalized183–223275–335+50%
Q&T 205°C420–515455–565+9%
Q&T 315°C390–480400–490+2%
Q&T 425°C345–420335–410-3%
Q&T 540°C285–355260–320-9%
Q&T 650°C225–275210–260-6%
AISI 4130 vs AISI 4140 Hardness (HV)4130 Annealed145–1854140 Annealed183–2234130 Normalized183–2234140 Normalized275–3354130 Q&T 205°C420–5154140 Q&T 205°C455–5654130 Q&T 315°C390–4804140 Q&T 315°C400–4904130 Q&T 425°C345–4204140 Q&T 425°C335–4104130 Q&T 540°C285–3554140 Q&T 540°C260–3204130 Q&T 650°C225–2754140 Q&T 650°C210–260

AISI 4130 vs AISI 4140 Elongation

ConditionAISI 4130 (%)AISI 4140 (%)AISI 4140 vs AISI 4130
Annealed22–3420–31-9%
Normalized5–1813.5–21.5+52%
Q&T 205°C8–126–10-20%
Q&T 315°C8.5–13.57–11-18%
Q&T 425°C10–1610–16+0%
Q&T 540°C13–2114–22+6%
Q&T 650°C17–2717–27+0%

AISI 4130 vs AISI 4140 Fracture toughness

ConditionAISI 4130 (MPa·m0.5)AISI 4140 (MPa·m0.5)AISI 4140 vs AISI 4130
Annealed75–12276–120-1%
Normalized72–11468–107-6%
Q&T 205°C29–5324–48-12%
Q&T 315°C30–5529–54-2%
Q&T 425°C34–6036–63+5%
Q&T 540°C43–7145–74+4%
Q&T 650°C48–7950–80+2%
AISI 4130 vs AISI 4140 Fracture toughness (MPa√m)4130 Annealed75–1224140 Annealed76–1204130 Normalized72–1144140 Normalized68–1074130 Q&T 205°C29–534140 Q&T 205°C24–484130 Q&T 315°C30–554140 Q&T 315°C29–544130 Q&T 425°C34–604140 Q&T 425°C36–634130 Q&T 540°C43–714140 Q&T 540°C45–744130 Q&T 650°C48–794140 Q&T 650°C50–80

AISI 4130 vs AISI 4140 Fatigue strength at 107 cycles

ConditionAISI 4130 (MPa)AISI 4140 (MPa)AISI 4140 vs AISI 4130
Annealed263–307297–341+12%
Normalized299–347402–465+34%
Q&T 205°C555–639593–684+7%
Q&T 315°C526–608540–622+2%
Q&T 425°C472–545463–535-2%
Q&T 540°C405–470383–442-6%
Q&T 650°C343–397326–379-5%

AISI 4130 vs AISI 4140 Machining speed

ConditionAISI 4130 (m/min)AISI 4140 (m/min)AISI 4140 vs AISI 4130
Annealed29.925-16%
Normalized24.415.8-35%
Q&T 205°C9.758.84-9%
Q&T 315°C10.410.4+0%
Q&T 425°C12.212.8+5%
Q&T 540°C14.916.8+13%
Q&T 650°C19.221.3+11%

AISI 4130 vs AISI 4140 Weldability, Processing and Corrosion

PropertyAISI 4130AISI 4140
WeldabilityGoodGood
Carbon equivalency0.537–0.70.695–0.867

AISI 4130 vs AISI 4140: Key Differences

On average across 7 matched conditions, AISI 4140 has 10% higher tensile strength than AISI 4130. On average across 7 matched conditions, AISI 4140 has 6% higher yield strength than AISI 4130. Fracture toughness is practically the same for AISI 4130 and AISI 4140 (average difference -1% across 7 matched conditions). On average across 7 matched conditions, AISI 4140 has 5% lower machining speed than AISI 4130. Elongation is practically the same for AISI 4130 and AISI 4140 (average difference +2% across 7 matched conditions).

AISI 4130 vs 4140 FAQ

Is 4140 stronger than 4130?

Yes. Across 7 matched conditions in our data sheets, AISI 4140 has on average about 10% higher tensile strength and 6% higher yield strength than AISI 4130. Note that our 4130 quenched and tempered data is for water quenching and the 4140 data for oil quenching.

What is the difference between 4130 and 4140 composition?

The main difference is carbon: AISI 4130 contains 0.28–0.33% carbon and AISI 4140 0.38–0.43%. Chromium (0.8–1.1%) and molybdenum (0.15–0.25%) are the same in both data sheets.

Which is easier to machine, 4130 or 4140?

Annealed AISI 4130 has a machining speed of 29.9 m/min and annealed AISI 4140 25 m/min in our data sheets, so 4130 machines faster.

Is 4130 or 4140 harder when annealed?

Annealed AISI 4130 is 145–185 HV and annealed AISI 4140 is 183–223 HV in our data sheets.

Which is tougher, 4130 or 4140?

Fracture toughness is practically the same on average across the matched conditions in our data (difference -1%). Annealed: 75–122 MPa·m^0.5 for 4130 vs 76–120 for 4140.

AISI 4130 and AISI 4140 Material Data Sheets

AISI 4130 Annealed | AISI 4130 Air Melted, Normalized | AISI 4130 Water Quenched & Tempered at 205°C | AISI 4130 Water Quenched & Tempered at 315°C | AISI 4130 Water Quenched & Tempered at 425°C | AISI 4130 Water Quenched & Tempered at 540°C | AISI 4130 Water Quenched & Tempered at 650°C | All AISI 4130 conditions

AISI 4140 Annealed | AISI 4140 Normalized | AISI 4140 Oil Quenched & Tempered at 205°C | AISI 4140 Oil Quenched & Tempered at 315°C | AISI 4140 Oil Quenched & Tempered at 425°C | AISI 4140 Oil Quenched & Tempered at 540°C | AISI 4140 Oil Quenched & Tempered at 650°C | All AISI 4140 conditions

Need AISI 4130 or AISI 4140 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined steel parts in-house, heat treated to the condition you specify, and inspects them before shipment.