AISI 1022 Annealed Material Data Sheet

AISI 1022 Annealed Material Data Sheet

AISI 1022 Annealed Overview

AISI 1022 annealed is AISI 1022 low carbon steel (UNS G10220, EN 2C22) in the annealed condition. This AISI 1022 annealed material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 1022 conditions in our AISI 1022 yield, tensile and hardness comparison. Looking for AISI 1022 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1022 steel parts in-house and inspects them before shipment.

AISI 1022 Annealed Designation

AISI 1022
ConditionAnnealed
UNS numberG10220
US nameASTM MTX1020, ASTM 1022, ASME G10220, ASME G10210, ~SAE 050W, ~SAE 045Z, ~SAE 045Y, ~SAE 045X, ~SAE 045W, ~SAE 040S, ~SAE 040C, ~SAE 040B, ~SAE 040A
EN name2C22, 055M15, ~S270GP
EN number~1.0023
ISO name~R44, ~HR275 Class B, ~E275 Quality A
GB (Chinese) name~ML22Mn
JIS (Japanese) name~SWRCH22A, ~STK500, ~SNR400A, ~SN 400 A, ~SM400A, ~SHK 400 M, ~SG 295

AISI 1022 Annealed Typical uses

General construction, general mechanical engineering, automotive, tools, axles, gears, springs.

AISI 1022 Annealed Composition detail

C (carbon)0.18–0.23%
Fe (iron)98.7–99.1%
Mn (manganese)0.7–1%
P (phosphorus)0–0.04%
S (sulfur)0–0.05%

AISI 1022 Annealed Physical properties

Density7.8–7.9g/cm3

AISI 1022 Annealed Mechanical properties

Young’s modulus205–215GPa
Specific stiffness26.1–27.4MN.m/kg
Yield strength (elastic limit)285–350MPa
Tensile strength380–475MPa
Specific strength36.3–44.6kN.m/kg
Elongation28–42% strain
Compressive strength285–350MPa
Flexural modulus205–215GPa
Flexural strength (modulus of rupture)285–350MPa
Shear modulus79–84GPa
Bulk modulus158–175GPa
Poisson’s ratio0.285–0.295 
Shape factor60
Hardness – Vickers130–160HV
Elastic stored energy (springs)195–289kJ/m3
Fatigue strength at 10^7 cycles217–255MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
186–297MPa

AISI 1022 Annealed Impact & fracture properties

Fracture toughness42–67MPa.m0.5
Toughness (G)8.78–20.5kJ/m2

AISI 1022 Annealed Thermal properties

Melting point1480–1520°C
Maximum service temperature340–356°C
Minimum service temperature-68–-43°C
Thermal conductivity50–54W/m.°C
Specific heat capacity465–505J/kg.°C
Thermal expansion coefficient12–13µstrain/°C
Thermal shock resistance108–135°C
Thermal distortion resistance3.94–4.4MW/m
Latent heat of fusion270–275kJ/kg

AISI 1022 Annealed Electrical properties

Electrical resistivity16–18µohm.cm
Electrical conductivity9.58–10.8%IACS
Galvanic potential-0.52–-0.44V

AISI 1022 Annealed Magnetic properties

Magnetic typeMagnetic

AISI 1022 Annealed Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5110–5240m/s
Mechanical loss coefficient (tan delta)0.00103–0.00128 

AISI 1022 Annealed Processing properties

Metal castingUnsuitable
Metal cold formingAcceptable
Metal hot formingExcellent
Metal press formingAcceptable
Metal deep drawingLimited use
Machining speed39.6 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good
Carbon equivalency0.297 – 0.397

AISI 1022 Annealed Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Aluminum bronze is the most suitable mating material to minimize galling.
Limited use
FlammabilityNon-flammable

AISI 1022 Annealed Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; Other susceptible environments: Nitrate, hydroxide, carbonate, ammonia
Not susceptible

AISI 1022 Annealed Standards with similar compositions

Argentina: IRAM 1018 to IAS
Canada: A to CSA B193, B193 to CSA B193
China: ML22Mn to GB/T 6478
India: 20C8 to IS 11169/1, 20C8 to IS 1570/2/1, C20 to IS 1570/2/1, Fe 380 to IS 12367, Grade 7M to IS 7887, Grade 7M to IS 8952, Grade 8M to IS 7887, Grade 8M to IS 8952
Japan: SWRCH22A to JIS G3507
Mexico: 1018 to NMX-B-301, 1019 to NMX-B-301, 1021 to NMX-B-301, 1022 to NMX-B-301, MTX1020 to NMX-B-201, MTX1020 to NMX-B-203-SCFI
Pan America: 1018 to COPANT 331, 1018 to COPANT 333, 1019 to COPANT 333, 1021 to COPANT 331, 1021 to COPANT 333, 1022 to COPANT 330, 1022 to COPANT 331, 1022 to COPANT 333
South Korea: SWRCH22A to KS D 3592
UK: 170H20 to BS 970/1
USA: 1018, 1018 Class A to ASTM A311/A311M, 1018 to ASTM A29/A29M, 1018 to ASTM A519, 1018 to ASTM A787, 1018 to FED QQ-S-698, 1018 to FED QQ-W-461H, 1018 to MIL-R-8814, 1018 to SAE J403, 1019, 1019 Mod, 1019 to ASTM A29/A29M, 1019 to ASTM A512-96, 1019 to ASTM A513, 1019 to ASTM A519, 1019 to ASTM A568/A568M, 1019 to ASTM A787, 1019 to FED QQ-S-633A, 1019 to SAE J1249, 1019 to SAE J403, 1021, 1021 to ASTM A29/A29M, 1021 to ASTM A512-96, 1021 to ASTM A513, 1021 to ASTM A519, 1021 to ASTM A568/A568M, 1021 to ASTM A787, 1021 to SAE J403, 1022, 1022 Mod, 1022 to ASTM A29/A29M, 1022 to ASTM A513, 1022 to ASTM A519, 1022 to ASTM A568/A568M, 1022 to DoD-F-24669/1, 1022 to SAE J403, 10L18, G10180 to ASTM A510/A510M, G10180 to ASTM A576-90b, G10180 to ASTM A830/A830M, G10190 to ASTM A510/A510M, G10190 to ASTM A576-90b, G10190 to ASTM A830/A830M, G10210 to ASTM A510/A510M, G10210 to ASTM A576-90b, G10210 to ASTM A830/A830M, G10220 to ASTM A510/A510M, G10220 to ASTM A576-90b, G10220 to ASTM A830/A830M, Grade B to ASTM A595, HT to MIL-S-16113, MIL-R-908 to MIL-R-908, MIL-S-20166 to MIL-S-20166B, MIL-S-7809 to MIL-S-7809, MTX1020 to ASTM A512-96, MTX1020 to ASTM A513, MTX1020 to ASTM A519, MTX1020 to ASTM A787, UNS G10180, UNS G10180 to UNS, UNS G10190, UNS G10190 to UNS, UNS G10210, UNS G10210 to UNS, UNS G10220, UNS G10220 to UNS, UNS K02005
Tradenames: AMERHEAD C-1018, GREDE 31, HI-YIELD 42, JESSOP A-3, LASALLE 1018, LASALLE 1020-90, MANGANESE SCREW STOCK, MARINER, MARREL 50SS, NO. 1020-90 STEEL, SANDVIK 4L7, SWB-22M3, TISCON, UGINE B21, USS 2090, USS B24