AISI 1020 As Rolled Material Data Sheet

AISI 1020 As Rolled Material Data Sheet

AISI 1020 As Rolled Overview

AISI 1020 as rolled is AISI 1020 low carbon steel (UNS G10200) in the as rolled condition. This AISI 1020 as rolled material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 1020 conditions in our AISI 1020 yield, tensile and hardness comparison. Looking for AISI 1020 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1020 steel parts in-house and inspects them before shipment.

AISI 1020 As Rolled Designation

AISI 1020
ConditionAs rolled
UNS numberG10200
US nameASTM MT1020, ASTM M1020, ASTM 1020, ASME G10200, ASME G10170, ASME 1017, ~SAE 040 X, Y, Z, ~SAE 035S, ~SAE 035C, ~SAE 035B, ~SAE 035A, ~SAE 035 X, Y, Z, ~ASTM A836, ~ASTM 1018 Class A, ~ASME G10210, ~ASME G10180, ~ASME 1021
EN nameS240GP, ~P355NB, ~P310NB, ~HS15
EN number~1.0021
ISO name~E235 Quality A, ~CE20E4, ~CC21A
GB (Chinese) name~ML20Al, ~ML18Mn
JIS (Japanese) nameSWRM 20, SWRCH20A, SG 255, ~SWRCH18A, ~STKM12C, ~STKM12B, ~STKM12A, ~SPHT 2

AISI 1020 As Rolled Typical uses

Forgings, machined parts, shafts, car wheel hubs, general haulage gear

AISI 1020 As Rolled Composition detail

C (carbon)0.17–0.23%
Fe (iron)99.1–99.5%
Mn (manganese)0.3–0.6%
P (phosphorus)0–0.04%
S (sulfur)0–0.05%

AISI 1020 As Rolled Physical properties

Density7.8–7.9g/cm3

AISI 1020 As Rolled Mechanical properties

Young’s modulus205–215GPa
Specific stiffness26.1–27.4MN.m/kg
Yield strength (elastic limit)295–365MPa
Tensile strength395–500MPa
Specific strength37.6–46.5kN.m/kg
Elongation28–43% strain
Compressive strength295–365MPa
Flexural modulus205–215GPa
Flexural strength (modulus of rupture)295–365MPa
Shear modulus79–84GPa
Bulk modulus158–175GPa
Poisson’s ratio0.285–0.295 
Shape factor59
Hardness – Vickers135–165HV
Elastic stored energy (springs)209–314kJ/m3
Fatigue strength at 10^7 cycles223–264MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
190–310MPa

AISI 1020 As Rolled Impact & fracture properties

Fracture toughness41–68MPa.m0.5
Toughness (G)8.43–20.9kJ/m2

AISI 1020 As Rolled Thermal properties

Melting point1480–1520°C
Maximum service temperature340–356°C
Minimum service temperature-68–-38°C
Thermal conductivity50–54W/m.°C
Specific heat capacity465–505J/kg.°C
Thermal expansion coefficient11.5–12.5µstrain/°C
Thermal shock resistance116–146°C
Thermal distortion resistance4.1–4.58MW/m
Latent heat of fusion270–275kJ/kg

AISI 1020 As Rolled Electrical properties

Electrical resistivity16–18µohm.cm
Electrical conductivity9.58–10.8%IACS
Galvanic potential-0.51–-0.43V

AISI 1020 As Rolled Magnetic properties

Magnetic typeMagnetic

AISI 1020 As Rolled Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5110–5240m/s
Mechanical loss coefficient (tan delta)9.8e-4–0.00124 

AISI 1020 As Rolled Processing properties

Metal castingUnsuitable
Metal cold formingAcceptable
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingAcceptable
Machining speed36.6 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good
Carbon equivalency0.22 – 0.33

AISI 1020 As Rolled Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Aluminum bronze is the most suitable mating material to minimize galling.
Acceptable
FlammabilityNon-flammable

AISI 1020 As Rolled Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; Other susceptible environments: Nitrate, hydroxide, carbonate, ammonia
Not susceptible

AISI 1020 As Rolled Standards with similar compositions

Australia: S1020 to AS 1442, S1020 to AS 1443, S1020 to AS 1446
Austria: C22SP to ONORM M3167
China: CRB650 to GB 13788, ML20Al to GB/T 6478, Q235 to GB/T 3524
Hungary: B38X to MSZ 500
India: 17C5 to IS 8053, ERW-3 to IS 3074, Grade 8 to IS 7887, Grade 8 to IS 8952
International: CC21A to ISO 4954
Italy: C21 to UNI 6922, CB20FF to UNI 7356
Japan: SWRCH20A to JIS G3507, SWRM 20 to JIS G3505
Mexico: 1020 to NMX-B-301, MT1020 to NMX-B-201, MT1020 to NMX-B-203-SCFI
Pan America: 1020 to COPANT 330, 1020 to COPANT 331, 1020 to COPANT 333
South Korea: SWRCH20A to KS D 3592, SWRM 20 to KS D 3554
Spain: 18KA-DF to UNE 36032, 20KA-DF to UNE 36032, F.7516 to UNE 36032, F.7517 to UNE 36032
UK: 040A20 to BS 970/1
USA: 1020, 1020 to ASTM A29/A29M, 1020 to ASTM A512-96, 1020 to ASTM A513, 1020 to ASTM A519, 1020 to ASTM A568/A568M, 1020 to DoD-F-24669/1, 1020 to FED QQ-S-635B, 1020 to FED QQ-S-698, 1020 to FED QQ-W-461H, 1020 to MIL-S-7952A, 1020 to MIL-T-3520, 1020 to SAE J403, 1023, 1023 to ASTM A513, 1023 to ASTM A568/A568M, 1023 to SAE J403, 5032 to AMS 5032E, C2 to MIL-S-16788A, CS1020 to MIL-S-11310E, G10200 to ASTM A510/A510M, G10200 to ASTM A576-90b, G10200 to ASTM A830/A830M, G10200 to MIL-S-46059, Grade A to ASTM A595, Grade B to ASTM A730, M1020, M1020 to ASTM A29/A29M, M1020 to ASTM A575-96, M1020 to SAE J403, MT1020 to ASTM A512-96, MT1020 to ASTM A513, MT1020 to ASTM A519, MT1020 to ASTM A787, UNS G10200, UNS G10200 to UNS, UNS G10230, UNS K01900, UNS K02000, UNS K02004, UNS K11900
Tradenames: ASCOMETAL XC18, B-W STANDARDIZED, CS1020, MARREL M5, POMPEY FFC 2, TOLEDO 15, UNION MC QUAID-EHN, V2