AISI 1020 Annealed Material Data Sheet
AISI 1020 Annealed Overview
| AISI 1020 annealed is AISI 1020 low carbon steel (UNS G10200) in the annealed condition. This AISI 1020 annealed material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 1020 conditions in our AISI 1020 yield, tensile and hardness comparison. Looking for AISI 1020 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1020 steel parts in-house and inspects them before shipment. |
AISI 1020 Annealed Designation
| AISI 1020 | |
| Condition | Annealed |
| UNS number | G10200 |
| US name | ASTM MT1020, ASTM M1020, ASTM 1020, ASME G10200, ASME G10170, ASME 1017, ~SAE 040 X, Y, Z, ~SAE 035S, ~SAE 035C, ~SAE 035B, ~SAE 035A, ~SAE 035 X, Y, Z, ~ASTM A836, ~ASTM 1018 Class A, ~ASME G10210, ~ASME G10180, ~ASME 1021 |
| EN name | S240GP, ~P355NB, ~P310NB, ~HS15 |
| EN number | ~1.0021 |
| ISO name | ~E235 Quality A, ~CE20E4, ~CC21A |
| GB (Chinese) name | ~ML20Al, ~ML18Mn |
| JIS (Japanese) name | SWRM 20, SWRCH20A, SG 255, ~SWRCH18A, ~STKM12C, ~STKM12B, ~STKM12A, ~SPHT 2 |
AISI 1020 Annealed Typical uses
| Forgings, machined parts, shafts, car wheel hubs, general haulage gear |
AISI 1020 Annealed Composition detail
| C (carbon) | 0.17 | – | 0.23 | % |
| Fe (iron) | 99.1 | – | 99.5 | % |
| Mn (manganese) | 0.3 | – | 0.6 | % |
| P (phosphorus) | 0 | – | 0.04 | % |
| S (sulfur) | 0 | – | 0.05 | % |
AISI 1020 Annealed Physical properties
| Density | 7.8 | – | 7.9 | g/cm3 |
AISI 1020 Annealed Mechanical properties
| Young’s modulus | 205 | – | 215 | GPa |
| Specific stiffness | 26.1 | – | 27.4 | MN.m/kg |
| Yield strength (elastic limit) | 265 | – | 325 | MPa |
| Tensile strength | 355 | – | 435 | MPa |
| Specific strength | 33.8 | – | 41.4 | kN.m/kg |
| Elongation | 28 | – | 43 | % strain |
| Compressive strength | 265 | – | 325 | MPa |
| Flexural modulus | 205 | – | 215 | GPa |
| Flexural strength (modulus of rupture) | 265 | – | 325 | MPa |
| Shear modulus | 79 | – | 84 | GPa |
| Bulk modulus | 158 | – | 175 | GPa |
| Poisson’s ratio | 0.285 | – | 0.295 | |
| Shape factor | 61 | |||
| Hardness – Vickers | 110 | – | 130 | HV |
| Elastic stored energy (springs) | 169 | – | 249 | kJ/m3 |
| Fatigue strength at 10^7 cycles | 207 | – | 240 | MPa |
| Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles | 180 | – | 277 | MPa |
AISI 1020 Annealed Impact & fracture properties
| Fracture toughness | 42 | – | 67 | MPa.m0.5 |
| Toughness (G) | 8.78 | – | 20.5 | kJ/m2 |
AISI 1020 Annealed Thermal properties
| Melting point | 1480 | – | 1520 | °C |
| Maximum service temperature | 340 | – | 356 | °C |
| Minimum service temperature | -68 | – | -43 | °C |
| Thermal conductivity | 50 | – | 54 | W/m.°C |
| Specific heat capacity | 465 | – | 505 | J/kg.°C |
| Thermal expansion coefficient | 11.5 | – | 12.5 | µstrain/°C |
| Thermal shock resistance | 104 | – | 130 | °C |
| Thermal distortion resistance | 4.1 | – | 4.58 | MW/m |
| Latent heat of fusion | 270 | – | 275 | kJ/kg |
AISI 1020 Annealed Electrical properties
| Electrical resistivity | 16 | – | 18 | µohm.cm |
| Electrical conductivity | 9.58 | – | 10.8 | %IACS |
| Galvanic potential | -0.51 | – | -0.43 | V |
AISI 1020 Annealed Magnetic properties
| Magnetic type | Magnetic |
AISI 1020 Annealed Optical, aesthetic and acoustic properties
| Transparency | Opaque | |||
| Acoustic velocity | 5110 | – | 5240 | m/s |
| Mechanical loss coefficient (tan delta) | 0.00111 | – | 0.00137 | |
AISI 1020 Annealed Processing properties
| Metal casting | Unsuitable |
| Metal cold forming | Acceptable |
| Metal hot forming | Excellent |
| Metal press forming | Excellent |
| Metal deep drawing | Acceptable |
| Machining speed | 45.7 m/min |
| Weldability Notes: Preheating and post weld heat treatments are required | Good |
| Carbon equivalency | 0.22 – 0.33 |
AISI 1020 Annealed Durability
| Water (fresh) | Acceptable |
| Water (salt) | Limited use |
| Weak acids | Limited use |
| Strong acids | Unacceptable |
| Weak alkalis | Acceptable |
| Strong alkalis | Limited use |
| Organic solvents | Excellent |
| Oxidation at 500C | Acceptable |
| UV radiation (sunlight) | Excellent |
| Galling resistance (adhesive wear) Notes: Aluminum bronze is the most suitable mating material to minimize galling. | Acceptable |
| Flammability | Non-flammable |
AISI 1020 Annealed Corrosion resistance
| Stress corrosion cracking Note: Rated in chloride; Other susceptible environments: Nitrate, hydroxide, carbonate, ammonia | Not susceptible |
AISI 1020 Annealed Standards with similar compositions
| Australia: S1020 to AS 1442, S1020 to AS 1443, S1020 to AS 1446 |
| Austria: C22SP to ONORM M3167 |
| China: CRB650 to GB 13788, ML20Al to GB/T 6478, Q235 to GB/T 3524 |
| Hungary: B38X to MSZ 500 |
| India: 17C5 to IS 8053, ERW-3 to IS 3074, Grade 8 to IS 7887, Grade 8 to IS 8952 |
| International: CC21A to ISO 4954 |
| Italy: C21 to UNI 6922, CB20FF to UNI 7356 |
| Japan: SWRCH20A to JIS G3507, SWRM 20 to JIS G3505 |
| Mexico: 1020 to NMX-B-301, MT1020 to NMX-B-201, MT1020 to NMX-B-203-SCFI |
| Pan America: 1020 to COPANT 330, 1020 to COPANT 331, 1020 to COPANT 333 |
| South Korea: SWRCH20A to KS D 3592, SWRM 20 to KS D 3554 |
| Spain: 18KA-DF to UNE 36032, 20KA-DF to UNE 36032, F.7516 to UNE 36032, F.7517 to UNE 36032 |
| UK: 040A20 to BS 970/1 |
| USA: 1020, 1020 to ASTM A29/A29M, 1020 to ASTM A512-96, 1020 to ASTM A513, 1020 to ASTM A519, 1020 to ASTM A568/A568M, 1020 to DoD-F-24669/1, 1020 to FED QQ-S-635B, 1020 to FED QQ-S-698, 1020 to FED QQ-W-461H, 1020 to MIL-S-7952A, 1020 to MIL-T-3520, 1020 to SAE J403, 1023, 1023 to ASTM A513, 1023 to ASTM A568/A568M, 1023 to SAE J403, 5032 to AMS 5032E, C2 to MIL-S-16788A, CS1020 to MIL-S-11310E, G10200 to ASTM A510/A510M, G10200 to ASTM A576-90b, G10200 to ASTM A830/A830M, G10200 to MIL-S-46059, Grade A to ASTM A595, Grade B to ASTM A730, M1020, M1020 to ASTM A29/A29M, M1020 to ASTM A575-96, M1020 to SAE J403, MT1020 to ASTM A512-96, MT1020 to ASTM A513, MT1020 to ASTM A519, MT1020 to ASTM A787, UNS G10200, UNS G10200 to UNS, UNS G10230, UNS K01900, UNS K02000, UNS K02004, UNS K11900 |
| Tradenames: ASCOMETAL XC18, B-W STANDARDIZED, CS1020, MARREL M5, POMPEY FFC 2, TOLEDO 15, UNION MC QUAID-EHN, V2 |