AISI 1060 Annealed vs As Rolled vs Normalized vs Oil Quenched & Tempered (205–650°C): Yield, Tensile & Hardness Compared

How do the AISI 1060 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength, hardness, elongation and machining speed of AISI 1060 medium carbon steel (UNS G10600) side by side for 8 conditions: annealed, as rolled, normalized, oil quenched & tempered at 205°C, oil quenched & tempered at 315°C, oil quenched & tempered at 425°C, oil quenched & tempered at 540°C, oil quenched & tempered at 650°C. All values are taken from the individual AISI 1060 material data sheets linked below.

AISI 1060 Yield, Tensile and Hardness by Condition

ConditionYield strength (MPa)Tensile strength (MPa)Hardness (HV)Elongation (%)Machining speed (m/min)
Annealed330–415550–700165–20518–2727.4
As Rolled430–535725–900220–27013–2120.4
Normalized375–465695–855210–26014–2221.6
Oil Quenched & Tempered at 205°C700–860990–1220290–36010–1614.9
Oil Quenched & Tempered at 315°C700–860990–1220290–36010–1614.9
Oil Quenched & Tempered at 425°C685–845965–1190280–35011–1715.5
Oil Quenched & Tempered at 540°C600–740865–1070250–31013–2117.4
Oil Quenched & Tempered at 650°C465–580720–880210–26018–2821.3

AISI 1060 Differences Compared with Annealed

The table below shows how much each AISI 1060 condition differs from the annealed condition, based on the mid-point of each range. Positive values mean higher strength, hardness or elongation.

ConditionYield strengthTensile strengthHardnessElongation
As Rolled+30%+30%+32%-24%
Normalized+13%+24%+27%-20%
Oil Quenched & Tempered at 205°C+109%+77%+76%-42%
Oil Quenched & Tempered at 315°C+109%+77%+76%-42%
Oil Quenched & Tempered at 425°C+105%+72%+70%-38%
Oil Quenched & Tempered at 540°C+80%+55%+51%-24%
Oil Quenched & Tempered at 650°C+40%+28%+27%+2%

AISI 1060 Strength and Hardness Charts

AISI 1060 Yield strength by condition (MPa)Annealed330–415As Rolled430–535Normalized375–465OQ&T 205°C700–860OQ&T 315°C700–860OQ&T 425°C685–845OQ&T 540°C600–740OQ&T 650°C465–580
AISI 1060 Tensile strength by condition (MPa)Annealed550–700As Rolled725–900Normalized695–855OQ&T 205°C990–1220OQ&T 315°C990–1220OQ&T 425°C965–1190OQ&T 540°C865–1070OQ&T 650°C720–880
AISI 1060 Hardness by condition (HV)Annealed165–205As Rolled220–270Normalized210–260OQ&T 205°C290–360OQ&T 315°C290–360OQ&T 425°C280–350OQ&T 540°C250–310OQ&T 650°C210–260

AISI 1060 Heat Treatment Key Points

The highest tensile strength of AISI 1060 in these data sheets is reached in the oil quenched & tempered at 205°C condition (990–1220 MPa). The softest condition is annealed (165–205 HV), with a machining speed of 27.4 m/min, which is usually preferred for machining and forming. For oil quenched AISI 1060, raising the tempering temperature from 205°C to 650°C lowers hardness from 290–360 HV to 210–260 HV, trading strength for toughness and ductility.

AISI 1060 Material Data Sheets

AISI 1060 Annealed | AISI 1060 As Rolled | AISI 1060 Normalized | AISI 1060 Oil Quenched & Tempered at 205°C | AISI 1060 Oil Quenched & Tempered at 315°C | AISI 1060 Oil Quenched & Tempered at 425°C | AISI 1060 Oil Quenched & Tempered at 540°C | AISI 1060 Oil Quenched & Tempered at 650°C | All AISI 1060 conditions

Looking for AISI 1060 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1060 steel parts in-house, heat treated to the condition you specify, and inspects them before shipment.