AISI 1022 Annealed vs As Rolled vs Normalized: Yield, Tensile & Hardness Compared

How do the AISI 1022 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength, hardness, elongation and machining speed of AISI 1022 low carbon steel (UNS G10220, EN 2C22) side by side for 3 conditions: annealed, as rolled, normalized. All values are taken from the individual AISI 1022 material data sheets linked below.

AISI 1022 Yield, Tensile and Hardness by Condition

ConditionYield strength (MPa)Tensile strength (MPa)Hardness (HV)Elongation (%)Machining speed (m/min)
Annealed285–350380–475130–16028–4239.6
As Rolled320–395450–555143–17328–4233.5
Normalized320–395430–535135–16527–4136.6

AISI 1022 Differences Compared with Annealed

The table below shows how much each AISI 1022 condition differs from the annealed condition, based on the mid-point of each range. Positive values mean higher strength, hardness or elongation.

ConditionYield strengthTensile strengthHardnessElongation
As Rolled+13%+18%+9%+0%
Normalized+13%+13%+3%-3%

AISI 1022 Strength and Hardness Charts

AISI 1022 Yield strength by condition (MPa)Annealed285–350As Rolled320–395Normalized320–395
AISI 1022 Tensile strength by condition (MPa)Annealed380–475As Rolled450–555Normalized430–535
AISI 1022 Hardness by condition (HV)Annealed130–160As Rolled143–173Normalized135–165

AISI 1022 Heat Treatment Key Points

The highest tensile strength of AISI 1022 in these data sheets is reached in the as rolled condition (450–555 MPa). The softest condition is annealed (130–160 HV), with a machining speed of 39.6 m/min, which is usually preferred for machining and forming.

AISI 1022 Material Data Sheets

AISI 1022 Annealed | AISI 1022 As Rolled | AISI 1022 Normalized | All AISI 1022 conditions

Looking for AISI 1022 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1022 steel parts in-house, heat treated to the condition you specify, and inspects them before shipment.