How do the AISI 4140 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength and hardness of AISI 4140 (UNS G41400, EN 42CrMo4) side by side for 7 conditions: Annealed, Normalized, Oil Quenched & Tempered at 205°C, Oil Quenched & Tempered at 315°C, Oil Quenched & Tempered at 425°C, Oil Quenched & Tempered at 540°C, Oil Quenched & Tempered at 650°C. All values are taken from the individual AISI 4140 material data sheets linked below.
AISI 4140 Yield, Tensile and Hardness by Condition
| Condition | Yield strength (MPa) | Tensile strength (MPa) | Hardness (HV) | Elongation (%) |
|---|---|---|---|---|
| Annealed | 370–460 | 595–720 | 183–223 | 20–31 |
| Normalized | 595–715 | 915–1130 | 275–335 | 13.5–21.5 |
| Oil Quenched & Tempered at 205°C | 1480–1810 | 1600–1950 | 455–565 | 6–10 |
| Oil Quenched & Tempered at 315°C | 1290–1580 | 1400–1710 | 400–490 | 7–11 |
| Oil Quenched & Tempered at 425°C | 1020–1260 | 1120–1380 | 335–410 | 10–16 |
| Oil Quenched & Tempered at 540°C | 750–920 | 855–1050 | 260–320 | 14–22 |
| Oil Quenched & Tempered at 650°C | 595–715 | 680–840 | 210–260 | 17–27 |
AISI 4140 Differences Compared with Annealed
The table below shows how much each condition differs from the annealed condition, based on the mid-point of each range. Positive values mean higher strength or hardness.
| Condition | Yield strength | Tensile strength | Hardness | Elongation |
|---|---|---|---|---|
| Normalized | +58% | +56% | +50% | -31% |
| Oil Quenched & Tempered at 205°C | +296% | +170% | +151% | -69% |
| Oil Quenched & Tempered at 315°C | +246% | +137% | +119% | -65% |
| Oil Quenched & Tempered at 425°C | +175% | +90% | +83% | -49% |
| Oil Quenched & Tempered at 540°C | +101% | +45% | +43% | -29% |
| Oil Quenched & Tempered at 650°C | +58% | +16% | +16% | -14% |
AISI 4140 Strength and Hardness Charts
AISI 4140 Heat Treatment Key Points
The highest tensile strength is reached in the oil quenched & tempered at 205°C condition (1600–1950 MPa). The softest condition is annealed (183–223 HV), which is usually preferred for machining and forming. Raising the tempering temperature from 205°C to 650°C lowers hardness from 455–565 HV to 210–260 HV, trading strength for toughness and ductility.
AISI 4140 FAQ
AISI 4140 (UNS G41400) is a low alloy steel containing 0.38–0.43% carbon, 0.8–1.1% chromium, 0.75–1% manganese and 0.15–0.25% molybdenum. It is used for heavy duty shafts, connecting rods, high tensile bolts, propeller shaft joints, track pins.
AISI 4140 chemical composition: C 0.38–0.43%; Cr 0.8–1.1%; Mn 0.75–1%; Mo 0.15–0.25%; P 0–0.035%; S 0–0.04%; Si 0.15–0.35%; balance iron (Fe).
The closest European (EN) equivalent of AISI 4140 is 42CrMoS4 and 42CrMo4 (material number 1.7227 and 1.7223).
The hardness of AISI 4140 ranges from 183–223 HV (annealed) to 455–565 HV (oil quenched & tempered at 205°C).
Annealed AISI 4140 has a tensile strength of 595–720 MPa and a yield strength of 370–460 MPa. The highest values are reached when oil quenched & tempered at 205°C: 1600–1950 MPa tensile and 1480–1810 MPa yield strength.
Yes. Normalized AISI 4140 has a tensile strength of 915–1130 MPa and a hardness of 275–335 HV, compared with 595–720 MPa and 183–223 HV annealed.
Tempering oil quenched AISI 4140 at 205°C gives 455–565 HV and 1600–1950 MPa tensile strength; at 650°C it drops to 210–260 HV and 680–840 MPa, while elongation rises from 6–10% to 17–27%.
Annealed AISI 4140 has a machining speed of 25 m/min, the highest of its conditions; AISI 4140 oil quenched & tempered at 205°C has the lowest, 8.84 m/min.
AISI 4140 has good weldability, with a carbon equivalent of 0.695–0.867.
The density of AISI 4140 is 7.8–7.9 g/cm³.
AISI 4140 Material Data Sheets
AISI 4140 Annealed | AISI 4140 Normalized | AISI 4140 Oil Quenched & Tempered at 205°C | AISI 4140 Oil Quenched & Tempered at 315°C | AISI 4140 Oil Quenched & Tempered at 425°C | AISI 4140 Oil Quenched & Tempered at 540°C | AISI 4140 Oil Quenched & Tempered at 650°C | All AISI 4140 conditions
Looking for AISI 4140 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 4140 steel parts in-house, heat treated to the condition you specify, and inspects them before shipment.