PARA 50% Glass Fiber Toughened Material Data Sheet
PARA 50% Glass Fiber Toughened (Polyarylamide) Material Data Sheet
PARA 50% Glass Fiber Toughened Overview
PARA 50% glass fiber toughened is a grade of polyarylamide (PARA), designated Polyarylamide (50% glass fiber, toughened). This PARA 50% glass fiber toughened material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PARA parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PARA parts in-house and inspects them before shipment.
PARA 50% Glass Fiber Toughened Designation
Polyarylamide (50% glass fiber, toughened)
Tradenames
Ixef
PARA 50% Glass Fiber Toughened Typical uses
Automotive, furniture, small appliances, lawn mowers, power tools, electrical contactors and switches, electrical motor components, cell phones, faucet components.
PARA 50% Glass Fiber Toughened Composition detail
Polymer
35
–
45
%
Impact modifier
5
–
15
%
Glass (fiber)
50
%
PARA 50% Glass Fiber Toughened Physical properties
Density
1.62
–
1.65
g/cm3
PARA 50% Glass Fiber Toughened Mechanical properties
Young’s modulus
14.2
–
17.8
GPa
Specific stiffness
8.68
–
10.9
MN.m/kg
Yield strength (elastic limit)
178
–
222
MPa
Tensile strength
180
–
220
MPa
Specific strength
109
–
136
kN.m/kg
Elongation
2.21
–
3.19
% strain
Elongation at yield
1.86
–
3.54
% strain
Compressive modulus
15.2
–
16.8
GPa
Compressive strength
228
–
252
MPa
Flexural modulus
14.5
–
17.4
GPa
Flexural strength (modulus of rupture)
270
–
329
MPa
Shear modulus
5.83
–
6.13
GPa
Shear strength
108
–
132
MPa
Bulk modulus
15.5
–
17.2
GPa
Poisson’s ratio
0.335
–
0.337
Shape factor
7.1
Hardness – Vickers
57
–
63
HV
Hardness – Rockwell M
184
–
204
Hardness – Rockwell R
184
–
204
Hardness – Shore D
98
–
102
Elastic stored energy (springs)
984
–
1570
kJ/m3
Fatigue strength at 10^7 cycles
76
–
84
MPa
PARA 50% Glass Fiber Toughened Impact & fracture properties
Fracture toughness
5.36
–
5.92
MPa.m0.5
Toughness (G)
1.72
–
2.31
kJ/m2
Impact strength, notched 23 °C
8.64
–
16.8
kJ/m2
Impact strength, unnotched 23 °C
66
–
97
kJ/m2
PARA 50% Glass Fiber Toughened Thermal properties
Melting point
259
–
281
°C
Glass temperature
78
–
92.2
°C
Heat deflection temperature 0.45MPa
237
–
258
°C
Heat deflection temperature 1.8MPa
210
–
230
°C
Vicat softening point
77
–
90
°C
Maximum service temperature
179
–
198
°C
Thermal conductivity
0.569
–
0.591
W/m.°C
Specific heat capacity
1240
–
1260
J/kg.°C
PARA 50% Glass Fiber Toughened Electrical properties
Electrical resistivity
2e20
–
5e21
µohm.cm
Electrical conductivity
3.45e-20
–
8.62e-19
%IACS
Dielectric constant (relative permittivity)
3.62
–
5.1
Dissipation factor (dielectric loss tangent)
0.0145
–
0.0381
Dielectric strength (dielectric breakdown)
18.5
–
31.5
MV/m
Comparative tracking index
400
–
450
V
PARA 50% Glass Fiber Toughened Magnetic properties
Magnetic type
Non-magnetic
PARA 50% Glass Fiber Toughened Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
2940
–
3310
m/s
Mechanical loss coefficient (tan delta)
0.0063
–
0.00696
PARA 50% Glass Fiber Toughened Absorption & permeability
Water absorption @ 24 hrs
0.14
–
0.24
%
Water absorption @ sat
1.4
–
1.9
%
Humidity absorption @ sat
0.79
–
1.1
%
PARA 50% Glass Fiber Toughened Processing properties