PARA 20% Glass Fiber Wear Grade Material Data Sheet
PARA 20% Glass Fiber Wear Grade (Polyarylamide) Material Data Sheet
PARA 20% Glass Fiber Wear Grade Overview
PARA 20% glass fiber wear grade is a grade of polyarylamide (PARA), designated Polyarylamide (20% glass fiber, wear grade). This PARA 20% glass fiber wear grade material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PARA parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PARA parts in-house and inspects them before shipment.
PARA 20% Glass Fiber Wear Grade Designation
Polyarylamide (20% glass fiber, wear grade)
Tradenames
Reny
PARA 20% Glass Fiber Wear Grade Typical uses
Automotive, furniture, small appliances, lawn mowers, power tools, electrical contactors and switches, electrical motor components, cell phones, faucet components.
PARA 20% Glass Fiber Wear Grade Composition detail
Polymer
80
%
Glass (fiber)
20
%
PARA 20% Glass Fiber Wear Grade Physical properties
Density
1.5
–
1.53
g/cm3
PARA 20% Glass Fiber Wear Grade Mechanical properties
Young’s modulus
7.2
–
8.98
GPa
Specific stiffness
4.75
–
5.93
MN.m/kg
Yield strength (elastic limit)
95.3
–
119
MPa
Tensile strength
107
–
130
MPa
Specific strength
62.9
–
78.6
kN.m/kg
Elongation
2.22
–
3.2
% strain
Elongation at yield
1.87
–
3.55
% strain
Compressive modulus
7.69
–
8.49
GPa
Compressive strength
135
–
149
MPa
Flexural modulus
5.94
–
7.11
GPa
Flexural strength (modulus of rupture)
154
–
188
MPa
Shear modulus
2.92
–
3.07
GPa
Shear strength
63.9
–
78.2
MPa
Bulk modulus
8.66
–
9.57
GPa
Poisson’s ratio
0.35
–
0.352
Shape factor
6.8
Hardness – Vickers
31
–
34
HV
Hardness – Rockwell M
157
–
174
Hardness – Rockwell R
157
–
174
Hardness – Shore D
92
–
96
Elastic stored energy (springs)
559
–
890
kJ/m3
Fatigue strength at 10^7 cycles
45
–
49.7
MPa
PARA 20% Glass Fiber Wear Grade Impact & fracture properties
Fracture toughness
4.67
–
5.16
MPa.m0.5
Toughness (G)
2.59
–
3.46
kJ/m2
Impact strength, notched 23 °C
4.76
–
9.24
kJ/m2
Impact strength, unnotched 23 °C
35
–
38
kJ/m2
PARA 20% Glass Fiber Wear Grade Thermal properties
Melting point
269
–
291
°C
Glass temperature
78
–
92.2
°C
Heat deflection temperature 0.45MPa
237
–
258
°C
Heat deflection temperature 1.8MPa
210
–
230
°C
Vicat softening point
77
–
90
°C
Maximum service temperature
188
–
207
°C
Thermal conductivity
0.471
–
0.482
W/m.°C
Specific heat capacity
1310
–
1340
J/kg.°C
Thermal expansion coefficient
28.3
–
29.7
µstrain/°C
Thermal shock resistance
391
–
533
°C
Thermal distortion resistance
0.016
–
0.0169
MW/m
PARA 20% Glass Fiber Wear Grade Electrical properties
Electrical resistivity
2e20
–
5e21
µohm.cm
Electrical conductivity
3.45e-20
–
8.62e-19
%IACS
Dielectric constant (relative permittivity)
3.45
–
4.86
Dissipation factor (dielectric loss tangent)
0.0181
–
0.0476
Dielectric strength (dielectric breakdown)
20.8
–
35.4
MV/m
Comparative tracking index
600
V
PARA 20% Glass Fiber Wear Grade Magnetic properties
Magnetic type
Non-magnetic
PARA 20% Glass Fiber Wear Grade Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
2180
–
2440
m/s
Mechanical loss coefficient (tan delta)
0.00984
–
0.0109
PARA 20% Glass Fiber Wear Grade Absorption & permeability
Water absorption @ 24 hrs
0.17
–
0.27
%
Water absorption @ sat
4
–
5.3
%
Humidity absorption @ sat
1.5
–
2.1
%
PARA 20% Glass Fiber Wear Grade Processing properties