PA46 50% Glass Fiber (Polyamide 46) Material Data Sheet
PA46 50% Glass Fiber Overview
PA46 50% glass fiber is a grade of polyamide 46 (PA46, nylon 46), designated Polyamide (Nylon) (Type 46, 50% Glass Fiber). This PA46 50% glass fiber material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA46 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA46 parts in-house and inspects them before shipment.
PA46 50% Glass Fiber Designation
Polyamide (Nylon) (Type 46, 50% Glass Fiber)
Tradenames
Hifill, Stanyl, Stanyl Diablo
PA46 50% Glass Fiber Typical uses
Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.
PA46 50% Glass Fiber Composition detail
Polymer
50
%
Glass (fiber)
50
%
PA46 50% Glass Fiber Physical properties
Density
1.62
–
1.65
g/cm3
PA46 50% Glass Fiber Mechanical properties
Young’s modulus
8.9
–
11.1
GPa
Specific stiffness
5.44
–
6.79
MN.m/kg
Yield strength (elastic limit)
142
–
178
MPa
Tensile strength
144
–
176
MPa
Specific strength
86.8
–
109
kN.m/kg
Elongation
4.1
–
5.9
% strain
Elongation at yield
3.45
–
6.55
% strain
Compressive modulus
9.5
–
10.5
GPa
Compressive strength
182
–
202
MPa
Flexural modulus
8.19
–
9.81
GPa
Flexural strength (modulus of rupture)
225
–
275
MPa
Shear modulus
3.63
–
3.82
GPa
Shear strength
86.4
–
106
MPa
Bulk modulus
10.1
–
11.1
GPa
Poisson’s ratio
0.329
–
0.343
Shape factor
6
Hardness – Vickers
46
–
50
HV
Hardness – Rockwell M
181
–
200
Hardness – Rockwell R
181
–
200
Hardness – Shore D
97
–
101
Elastic stored energy (springs)
1000
–
1610
kJ/m3
Fatigue strength at 10^7 cycles
60.8
–
67.2
MPa
PA46 50% Glass Fiber Impact & fracture properties
Fracture toughness
4.87
–
5.38
MPa.m0.5
Toughness (G)
2.28
–
3.04
kJ/m2
Impact strength, notched 23 °C
16.3
–
31.7
kJ/m2
Impact strength, notched -30 °C
8.82
–
19.2
kJ/m2
Impact strength, unnotched 23 °C
89.1
–
131
kJ/m2
Impact strength, unnotched -30 °C
80
–
120
kJ/m2
PA46 50% Glass Fiber Thermal properties
Melting point
284
–
306
°C
Glass temperature
71
–
79
°C
Heat deflection temperature 0.45MPa
284
–
340
°C
Heat deflection temperature 1.8MPa
258
–
313
°C
Maximum service temperature
73
–
87
°C
Minimum service temperature
-58
–
-38
°C
Thermal conductivity
0.597
–
0.621
W/m.°C
Specific heat capacity
1240
–
1290
J/kg.°C
Thermal expansion coefficient
27.5
–
28.1
µstrain/°C
Thermal shock resistance
493
–
672
°C
Thermal distortion resistance
0.0214
–
0.0224
MW/m
PA46 50% Glass Fiber Electrical properties
Electrical resistivity
2e15
–
5e16
µohm.cm
Electrical conductivity
3.45e-15
–
8.62e-14
%IACS
Dielectric constant (relative permittivity)
13.3
–
18.7
Dissipation factor (dielectric loss tangent)
0.33
–
0.87
Dielectric strength (dielectric breakdown)
14.8
–
25.2
MV/m
Comparative tracking index
325
–
375
V
PA46 50% Glass Fiber Magnetic properties
Magnetic type
Non-magnetic
PA46 50% Glass Fiber Optical, aesthetic and acoustic properties