PA66 40% Long Carbon Fiber Material Data Sheet

PA66 40% Long Carbon Fiber (Polyamide 66) Material Data Sheet

PA66 40% Long Carbon Fiber Overview

PA66 40% long carbon fiber is a grade of polyamide 66 (PA66, nylon 66), designated Polyamide (Nylon) (Type 66, 40% Long Carbon Fiber). This PA66 40% long carbon fiber material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA66 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA66 parts in-house and inspects them before shipment.

PA66 40% Long Carbon Fiber Designation

Polyamide (Nylon) (Type 66, 40% Long Carbon Fiber)
TradenamesComplet, Onforce, Strator, Witcom

PA66 40% Long Carbon Fiber Typical uses

Automotive applications, boat parts, bicycle parts, pumps, power tools, structural parts

PA66 40% Long Carbon Fiber Composition detail

Polymer60  %
Carbon (fiber)40  %

PA66 40% Long Carbon Fiber Physical properties

Density1.28–1.35g/cm3

PA66 40% Long Carbon Fiber Mechanical properties

Young’s modulus29–38GPa
Specific stiffness22–29MN.m/kg
Yield strength (elastic limit)276–310MPa
Tensile strength297–320MPa
Specific strength209–237kN.m/kg
Elongation1–1.5% strain
Compressive modulus19.4–20.4GPa
Compressive strength343–400MPa
Flexural modulus22.7–28.5GPa
Flexural strength (modulus of rupture)414–460MPa
Shear modulus12.3–12.9GPa
Shear strength171–200MPa
Bulk modulus32.4–34GPa
Poisson’s ratio0.315–0.328 
Shape factor8.9
Hardness – Vickers68–75HV
Hardness – Shore D103–114 
Elastic stored energy (springs)1080–1530kJ/m3
Fatigue strength at 10^7 cycles78.4–91.5MPa

PA66 40% Long Carbon Fiber Impact & fracture properties

Fracture toughness11.7–14.2MPa.m0.5
Toughness (G)4.02–6.26kJ/m2
Impact strength, notched 23 °C15–26.9kJ/m2
Impact strength, notched -30 °C14.9–18.1kJ/m2
Impact strength, unnotched 23 °C50–110kJ/m2

PA66 40% Long Carbon Fiber Thermal properties

Melting point242–282°C
Glass temperature54–66°C
Heat deflection temperature 0.45MPa255  °C
Heat deflection temperature 1.8MPa246–250°C
Vicat softening point240–255°C
Maximum service temperature107–127°C
Minimum service temperature-81–-71°C
Thermal conductivity0.989–1.03W/m.°C
Specific heat capacity1410–1470J/kg.°C
Thermal expansion coefficient19  µstrain/°C
Thermal shock resistance401–536°C
Thermal distortion resistance0.0521–0.0542MW/m

PA66 40% Long Carbon Fiber Electrical properties

Electrical resistivity2e9–5e10µohm.cm
Electrical conductivity3.45e-9–8.62e-8%IACS
Galvanic potential0.14–0.22V

PA66 40% Long Carbon Fiber Magnetic properties

Magnetic typeNon-magnetic

PA66 40% Long Carbon Fiber Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity4680–5400m/s
Mechanical loss coefficient (tan delta)0.00399–0.00528 

PA66 40% Long Carbon Fiber Absorption & permeability

Water absorption @ 24 hrs0.51–0.83%
Water absorption @ sat5.1  %
Humidity absorption @ sat1.5–1.7%

PA66 40% Long Carbon Fiber Processing properties

Polymer injection moldingLimited use
Polymer extrusionUnsuitable
Polymer thermoformingLimited use
Linear mold shrinkage0.1 – 0.3 %
Melt temperature275 – 320 °C
Mold temperature80 – 170 °C
Molding pressure range69 – 138 MPa

PA66 40% Long Carbon Fiber Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisAcceptable
Organic solventsExcellent
Oxidation at 500CUnacceptable
UV radiation (sunlight)Poor
FlammabilitySlow-burning